Reading view

Best Knife Steel of Every Decade

Patreon

Thanks to my new Patreon supporters for supporting knife steel research! Magellan117, 許晉誠, Nathaniel Walker, Mark, Christopher Thomas, Joab Stecher, Steven Lagace, Francisco, Adam Lowenstein, Chantal, Timothy P Wright, John Schmidt, DiSH, diddybob, Andy Orsburn, Kfir Behar, John, Jacob Knudsen, and Jacob E. You can also become a supporter at Patreon.com/Knifesteelnerds.

Video

There is a video version of the following article:

History of Knife Steel

I love learning how different steels were developed and which knife companies and knifemakers chose to apply them to knives. I did a huge amount of research for my book, The Story of Knife Steel, which covered all the “stories” about how all of that happened. If you want to know where I got the different dates and background information in the article below then read The Story of Knife Steel.

This article was originally twice as long as it is because I wanted so badly to include so many stories and tidbits, but to keep it manageable, I had to cut most of that. If you want to get all of that missing content, then read the book. There are also tons of pictures of old knives and fun ads for steels of years past.

1981 ad for CPM-10V

Choosing Best Knife Steels by Decade

Below I have a table showing steels that were released in order of date, along with an approximate composition. You may notice that many of these steels were released quite a long time before they were actually used in knives. That is often because knifemakers didn’t learn about them until much later, though another important factor is that they often weren’t available in thin sheet and weren’t available in small quantities. So in this article I will be discussing what the best steels were that were actually being used in each decade, and what the best steels could have been if they had been popular in knives.

Knife Steel in the 1800s

In terms of alloys, by far the most common cutlery steel in the 1800s was simple high carbon steel. It is often reported that this was 1095 steel though it would be more properly called W1 tool steel. The differences are that W1 was somewhat lower in Mn, and also the carbon content for cutlery steel was sometimes higher than the 1095 spec allows (0.9-1.03% C). But they are similar enough that it is probably splitting hairs.

There was some experimentation with different steel alloys in knives, however. At the 1874 Mechanics’ Fair, the San Francisco knife companies Will & Finck and Michael Price were advertising their knives to be using “chrome steel.” This was presumably because of the hype of the Adamantine chromium steel developed by Julius Baur in the late 1860s. However, there were some knife companies advertising their knives to be using “chrome steel” when the steel in fact did not contain chromium. Assuming the San Francisco companies were actually using a chromium-alloyed steel, this was the first record of alloy steel being used in knives that I have found.

Michael Price carving set (unknown steel)

What Were the Best Knife Steels in the 1800s?

So before the 1870s the best knife steel choice was also the most popular, a simple high carbon steel made with the crucible method. Post-1870 the option of chromium steel was an interesting one, and probably would have been slightly superior to the simple carbon steels. That would offer a bit more wear resistance, better resistance to overheating in heat treatment, and also could be quenched more slowly and achieve full hardness. Mushet special steel was probably too extreme at the time, though it would be interesting to see an 1870s-era blade with that grade.

By the 1890s they would have technically also had access to F2 or CYW Choice, though I am not aware of any knifemakers actually using them. F2 has been used sporadically in knives over the years, offering a unique combination of being low hardenability (easier for forging or simple heat treating) along with relatively high wear resistance from the tungsten content. CYW Choice would also be very interesting, offering air hardening and wear resistance from its high chromium content. Chromium carbides are significantly harder than iron carbides. After all, the similar A2 makes an excellent knife steel, so CYW Choice could likely also work well.

Knife Steel in 1900-1939

Despite the rise of many alloy steels, simple carbon steel like W1 continued to be the dominant choice for decades to come. There were some exceptions, however.  Canton Cutlery began advertising vanadium-alloyed knife steel branded as “Car-Van Steel,” similar to W2. W.R. Case began purchasing “chrome vanadium” cutlery steel from Universal in December 1913 and Crucible Steel in 1915. I found a list of cutlery steel compositions from 1926 which included the simple carbon W1 types, 0.75% Cr alloyed types called “Chrome steel” and the 0.5% Cr, 0.2% V “chrome-vanadium” types. These 1926 compositions are very similar to steels used in more recent decades like 1095CV. The relatively common 80CrV2 is also similar to these grades but with 0.8% carbon.

The biggest alloy discovery in the early 1900s for knives was stainless steel, first developed by Harry Brearley in 1912. This early version was similar to the modern 420 stainless with about 0.3% C and 13% Cr. This steel was poorly regarded for its low hardness, and soon there were alternatives like 440A (1924), 440C (1925) and AEB (1925). Note this AEB is now called AEB-H, not the more common AEB-L; it had much higher carbon at 1% along with 14% Cr. Another important stainless was a steel called V3M in Germany (1922) which had higher carbon than 420 with 0.4% along with 14% Cr. This German steel would become the German specification called 1.4034, similar to the American 420HC.

The pickup of stainless outside of “table cutlery” like carving knives and forks was very slow, however. First, World War I essentially put a halt to stainless steel until 1919. But after that, the cutlery companies didn’t like stainless because it was more challenging to forge, heat treat, grind, and polish. It required a wholesale change to the processing and many companies did not want to make modifications to their setup. It became common for people to claim that stainless steel had worse edge retention than carbon steels. By the 1930s, 90% of table cutlery was stainless but only 10% of pocket knives.

440A (as it was later called) became known as the “hard cutlery type” which was used for its superior hardness and wear resistance than 420. 440A was sold under various names such as Latrobe Hy-glo, Firth-Sterling “Stainless B,” or Crucible “Rezistal Grade B.”  While I have found several references to these steels in the 1920s and 1930s, it was very rare back then to advertise specific steel types in knives. I tested a Schrade knife with a stamp from 1920s-1946 that had high enough chromium to be 440A. And a 1926 Schrade catalog implied they had recently switched to an improved stainless steel. A Remington 1937 sales manual also listed out information about their two stainless types, one a 420 and one a 440A/440B. I also tested a 1950-1964 W.R. Case knife that tested as 440, despite Case being best known for using 420HC in recent decades. I have also seen claims that Queen Cutlery was the first to use 440-type stainless steels but after investigating it I don’t think they were doing so until 1946.

One of the big advantages of using 440A or 440B vs the earlier 420 stainless was hardness. 420 was limited to the low 50s HRC while 440A could be heat treated as high as 59 HRC. And while 59 sounds relatively low today, the majority of carbon steel knives were around 56 HRC back then so the 440A was often being heat treated to a similar hardness.

Best Knife Steels in 1900-1939

While W1 continued to be the dominant choice, I would have preferred “chrome steel” or especially “chrome vanadium” steel for the slightly improved properties. 52100 was only really used in bearings, and O1 in tools in the early 1900s, but those would have been excellent choices as well. The high carbon, high chromium D3 tool steel has been used in small quantities in knives from the 1960s onward but it is too brittle for my taste. D2 has been a mainstay in the knife world, of course, but was not used in knives for several decades after its introduction in 1927. I don’t think high speed steels are the best choice for knives, but M2 after 1938 was a decent option. Gerber was famously using old hacksaw blades, which were first T1 steel and later M2, but that also wasn’t until 1938 at the earliest when David Z. Murphy began making knives.

For knifemakers preferring low alloy steels, my preference would be chrome steel in the very early 1900s, followed by 52100 after its introduction in 1905 if we are using revisionist history (the earliest record of 52100 in knives was the 1940s by Scagel during WWII steel shortages). After 1921 I would also like O7 tool steel for its wear resistance which is essentially chrome-vanadium steel plus 1.3% tungsten. For high alloy steels options CYW Choice would have been best starting in 1900, followed by D2 in 1927 and A2 in 1938, with an honorable mention for M2 after 1938 for high wear resistance.

Knife Steel in 1940-1989

Individual custom knifemakers were relatively rare in the early-to-mid 1900s, though there was an uptick during WWII. The most famous of these makers was Bo Randall who made his knives using O1 tool steel and 440B stainless.

Hoyt Buck of Buck Knives first started making knives out of used files (simple high carbon steel) after Pearl Harbor. This would evolve into a commercial factory knife company in the early 1960s where they used 440C because they were making too many knives to stick with old files. They switched to 425 Modified stainless steel in 1981 so that blanking was easier.

Gerber Knives would restart in 1945. They used old T1 hacksaw blades until 1948 because new hacksaw blades had a mild steel body with hardened steel teeth. At that point they would switch to M2 high speed steel supplied by Crucible Steel.

1950 Gerber ad

Gerber would expand into one of the largest and most respected commercial knife companies. They built a new factory in 1966. They added a new pocket knife called the Fh or Folding Hunter in 1968 in 440C stainless steel. This is the first commercial knife I know of that advertised a specific steel type:

1968 Gerber ad

Rise of Custom Knives

In the 1960s and 1970s there was a big increase in the number of custom knifemakers. A.G. Russell brought those makers together leading to the formation of the Knifemakers Guild in 1970.

1970 A.G. Russell ad featuring Loveless knife

Most knifemakers were advertising the specific steel type they were using, even in this period. The most popular steels in 1973 were O1, A2, W2, D2, O6, 440C, and 154CM. By 1971 440C stainless was perceived as being the best stainless but still falling short of non-stainless steels. Early users of 440C included D.E. Henry in 1960 and Gil Hibben in 1963; both of them mentioned having to purchase round bar and forge it flat. D2 had a reputation for having better properties than 440C but was not truly stainless. Early users of D2 in knives included Jimmy Lile and Chubby Hueske, who both started using it around 1968. In the fall of 1971 Loveless started using the bearing stainless steel 154CM and this grade became very popular.

From a different perspective of makers like Loveless using “new” fancy steels like 154CM were the forging smiths like Bill Moran who advertised the use of simple steels that were forged. Moran promoted that the forged blade was superior and that stainless steels did not benefit from the process. Moran’s focus on the past and recreating legendary blades led to his reintroduction of pattern-welded Damascus steel to the market in 1973, which were advertised as having superior properties in addition to the beautiful patterns. Damascus steel inspired many more makers to take up forging, leading to the formation of the American Bladesmith Society in 1976. I wrote more about the different philosophy of new steels with stock removal vs carbon steels with forging in this article.

Bob Schrimsher was the earliest to start a dedicated knife supply company in 1969. Before that A.G. Russell was supplying steel and handle materials. The steels that knifemakers use has historically been closely tied to what is available from knife supply companies. Especially back then it was not feasible for a knifemaker to call a steel company and order because they couldn’t purchase the minimum required amounts.

Custom Knives Inspiring Factory Companies

The growing custom knife market had more and more influence on factory knives. This led to Schrade working with Bob Loveless on what would become the first “factory collaboration” knife released in 1975. This was also the first factory knife to feature 154CM steel.

Ted Dowell would popularize Vasco Wear steel in knives after he learned about the steel from Bernard Sparks. Dowell began advertising the steel in 1977. This would influence Gerber, which would also use Vasco Wear in the FS II knives from 1982-1988.

Rise of Japan

Japanese factory knives gained more and more influence over the market starting in the 1970s. Pete Kershaw, a Gerber salesman, left to form his own company in 1974. These knives were marketed in 1976 as “Kai stainless” and in 1978 as “high carbon Kai stainless steel blade from the AUS series is an improvement over famous 440-C.” These were the grades AUS-6 and AUS-8A made in Japan.

1980s Al Mar SERE. Photo from Arizona Custom Knives.

154CM began to develop a reputation for being “dirty” with a high impurity content. Knife deal Okayasu Kazuo spoke to Hitachi and learned that they already made a version of 154CM called ATS-34. This steel was both cheaper and cleaner than 154CM and became the dominant custom knife steel in the 1980s and 1990s. The first factory knives available in the steel came from Al Mar knives produced in Japan in 1984.

Best Knife Steels 1940-1989

Factory knives largely continued to use 420, 440A, and simple carbon steel through the 1940s and 1960s. Some companies like Gerber and Buck began using 440C in the 1960s. And factory knives expanded into AUS-6/AUS-8A and ATS-34 after that.

Custom makers started with low alloy steels like O1 and W2 or high alloy steels like D2 and 440C. But 154CM and pattern-welded Damascus were the big turning points for what became popular in the early 1970s. There were also some intriguing less common options like Vasco Wear, however.

But in terms of what would have been truly best if it had been known and available is also an interesting question. 12C27 and AEB-L came out in the 1960s and those would have been good alternatives for high toughness. It wasn’t until the 2010s that AEB-L really began to take off in the custom knife world. BG42 also came out early, in 1961, and didn’t gain much popularity until the late 1990s, though I’m not sure it is a pure upgrade over 154CM.

1981 Blade Magazine ad for Uddeholm AEB-L

Other interesting choices would have been CPM-M4, released in 1973. Tim Wright first used it in 1980 but it didn’t become popular until the mid-2000s. That would have had superior properties to many of the conventional alloys being used in the 1970s and 1980s. And CPM-10V released in 1978 would have had higher wear resistance than any other steel on the market while still maintaining good toughness. The earliest case of its use I found was Ralph Turnbull in the early 1980s. Abrasives were not very good then and Turnbull reported that getting a good finish was nearly impossible.

Near the end of our 1940-1989 range there was the stainless CPM-440V (S60V). It was an interesting choice that didn’t gain any real popularity until the mid-to-late 1990s, which we will discuss in the next sections.

Knives and Steel in 1990-2001

In terms of steel developments there were a few interesting ones that largely didn’t get used in this decade. These included Elmax released in 1990, and M390 released in 1992. M390 in particular gained popularity much later, but initially was not pushed by Bohler as a knife steel. Later in the decade there was CPM-420V (later S90V) released around 1997, and CPM-3V released around 1999. In 2000 Crucible would change the name of CPM-440V to CPM-S60V and CPM-420V to CPM-S90V.

In terms of knives this was one of the oddest decades for knife steel, at least to me. ATS-34 continued to be the most popular choice into the 90s; if you include 154CM this was quite a long period of dominance for the steel. Despite BG42 being nearly as old as 154CM, it didn’t start to gain much popularity in knives until the mid-90s. Chris Reeve, inspired by Ted Dowell’s use of BG42, had called Latrobe Special Steel and convinced them to roll it into the right size for his knives which led to the wider availability. Factories like Buck and SOG offered it in knives shortly afterward. Knife supply companies like Tru-Grit were offering it in 1998, which also increased its popularity among custom knifemakers.

Chris Reeve small Sebenza in BG42. Photo by KnifeTreasures.com

Another alternative to the increasing price and decreasing availability of ATS-34 was to go back to the original – 154CM. Crucible Steel began making it in thin sheet again, providing a source for USA-made steel.

Spyderco introduced VG-10 into its Japanese-made knives starting in 1997. Ironically the first knife to use this steel was a fixed blade designed by Bill Moran, a knifemaker who famously did not like stainless steel. VG-10 would become a mainstay with Spyderco knives for years to come.

In the mid-90s Crucible’s CPM-440V (S60V) became more commonly available and its popularity steadily, though slowly, increased. The primary complaints about this steel were the difficulty in finishing, with the secondary complaint being toughness. Abrasives available to knifemakers and knife companies were not well suited to the high vanadium content of the grade. The recommended heat treatments were also poor, in my opinion, generally resulting in about 56-57 HRC.

Custom knifemaker Phil Wilson wrote many articles about knife steels in the mid-90s through the 2000s and he reported obtaining some CPM-420V around 1997. He said that the steel was even more difficult to finish than 440V but would cut longer, had higher toughness, and was easier to heat treat to higher hardness. Microtech would add it as an upcharge option starting in 2000.

Phil Wilson fillet knife

Best Knife Steels in 1990-2001

Two steels I think could have done well in this time period were Elmax and M390, released early on in the 1990s but didn’t get much use in knives until much later. They have a much lower content of hard vanadium carbides so the knife companies wouldn’t have had as many issues finishing them with the abrasives which were then available. Those steels would have also had superior toughness and edge retention to BG42.

I do like the steels CPM-440V and CPM-420V, S60V and S90V, however. It seems, like Marty McFly once said, that they weren’t “ready for that yet.” S90V has similar toughness to Elmax and M390 but with significantly greater wear resistance. But that greater wear resistance was also one of its biggest barriers to being used more frequently.

CPM-3V also has excellent toughness with good wear resistance, but it didn’t catch on widely at that time, perhaps because it is non-stainless.

Knives and Steel in 2002-2019

A huge moment in knife steel was the release of CPM-S30V in 2002. This was the culmination of Crucible Steel’s continued interest in the knife market. Dick Barber and Ed Severson of Crucible would go to Chris Reeve and ask him what they could do to get him to move from BG42 to their steel. He told them that S60V and S90V had too much vanadium for him to easily work with them, but he would switch if they could give him an improvement over BG42 that he could machine and grind. The new steel was advertised as being designed “specifically for knives” and took off basically immediately.

2002 article on S30V by Phil Wilson

After S30V, the other 90s “alternative” grades like BG42, S60V, and S90V basically went away in the knife world. Almost every knife company switched to the new steel. By 2003, S30V was the top selling knife steel from Crucible.

CPM-M4 would also build in popularity in this time period, especially in competition chopping knives for the new Blade Sports competitions. It would develop a reputation for having an excellent combination of properties including both toughness and wear resistance, though was not stainless.

Chris Reeve would request a new steel with improved machinability over S30V which led to the release of CPM-S35VN by Crucible around 2009. This would take over from S30V with a lot of knife companies after that. S35VN also had significantly higher toughness than S30V though at the cost of a little wear resistance.

Bohler-Uddeholm began pushing their steels in the USA, including N690, M390 and Elmax. They also pushed their version of D2, Vanadis 4 Extra, Vanax, K294, and K390, though with less success. K390 would become more popular a bit later after Spyderco began using it. M390 would be the main winner out of this group in terms of popularity, serving as an alternative to S30V and S35VN.

2011 Blade Magazine ad for Uddeholm Vanax

Kershaw would start using Sandvik’s 13C26 steel in their blanked knives made in their USA factory. They were unhappy with the corrosion resistance which led to Sandvik developing the improved 14C28N in 2009.

There were powder metallurgy versions of Vasco Wear coming out in this period, including Carpenter’s PD#1 in 2001, Zapp Z-Wear in 2010, and CPM-CruWear in 2013.

Spyderco would also introduce Zapp LC200N into their knives in 2013. This steel dates back to 1993 under the initial name of Cronidur 30.

Best Steels in 2002-2019

S30V, S35VN, and M390 were the big winners in this time period. In hindsight I don’t think S30V was really an improvement over the earlier Elmax and M390, but those steels were not generally available in sheet for knives. S35VN has better toughness than S30V, Elmax, or M390 which gives it more of a niche that is relevant.

For a non-PM less expensive stainless steel I think that 14C28N was a meaningful improvement over 13C26 and AEB-L, having higher corrosion resistance with otherwise similar properties.

Vanadis 4 Extra was a well balanced PM non-stainless steel introduced around 2004 but it didn’t really take off. The more available CPM-M4 offered similar properties, with somewhat better wear resistance and somewhat worse toughness.

Conclusions and Summary

For the table below I didn’t include any steel for a particular decade unless it came out early in the decade. In other words, if it came out in 1993 or before, it counts for that decade, but 1994 would not. This is not a comprehensive chart for everything so there is plenty left out but gives a summary of some of my thoughts above. Normally, I would want a full range of recommendations based on cost, manufacturing method, and the toughness-wear-resistance balance.

So I hope you have seen how messy the history can be, with large gaps between a new steel being released and it actually seeing use in knives. And there were many periods when better steels were available than what was being used. It is fun to look at hypothetical scenarios where CYW Choice would be used in knives starting in the 1890s, or CPM-M4 would have been popular with the new growing custom knife market of the 1970s, or if M390 and Elmax were popular throughout the 1990s.

The post Best Knife Steel of Every Decade appeared first on Knife Steel Nerds.

  •  

Carpenter A-421 Knife Steel

I am supposed to be getting some of this steel soon but I wanted to write up an analysis of the composition first. There was an article from BladeHQ about the steel and also a video from TKell Knives so I have gotten some questions about it.

Background

I was able to talk to Robert Buck, the developer of these steels, so when I got an answer to questions I had I will provide it, otherwise the following is my own analysis and speculation and shouldn’t be construed as anything official. Thank you Dr. Buck for speaking to me about the steel!

Carpenter’s A-421 knife steel actually started out as A-21 steel, which is the only version of the product that currently has a page on Carpenter’s website: https://www.carpentertechnology.com/alloy-finder/a-21

Here is the composition of A-21 according to the data sheet:

There are a bunch of ranges and maximums so here is the simplified composition using averages of each range. I also included A-421 which is the same apart from the carbon content. I will explain where I came up with the carbon content of A-421 shortly.

These grades were developed by Robert Buck, with A-21 patented in 2005 [1] and A-421 patented in 2024 [2]. I also found that Dr. Buck patented another steel in 1994 that is similar to A-21 but with a significant cobalt addition [3]. I asked Dr. Buck if this cobalt-alloyed version was ever commercially produced but he said that A-21 was the first to be available. The main unique thing that is discussed in each of these patents is the use of titanium. Titanium is relatively common in modern low alloy steels as a microalloy element, typically under 0.1%. It is relatively rare in tool steels and knife steels, however. Titanium forms a hard TiC carbide that can contribute to wear resistance in a similar way to adding niobium (Nb) or vanadium (V). The precursor patent says [3] that the titanium addition and the resulting TiC are used because they are “much smaller than the relatively large (0.1-0.3 μm) Cr-rich carbides” that they “precipitate homogeneously throughout the bulk material, rather than primarily on lath or grain boundaries,” and that they “do not coarsen appreciably during long term holds at high creep temperatures to about 700°C. Thus, the average interparticle spacing is small and remains so during creep.”

A-21 Stainless Steel and Titanium

A-21 was designed to be a martensitic stainless steel that is “fine-grained” due to the “relatively uniform dispersion of coarsening-resistant, MXX-type precipitates.” In other words, to have a small grain size due to TiC. A dispersion of small, stable carbides will “pin” grain boundaries thus slowing their growth and keeping the grain size small. Titanium can be a good element for this because the carbides will not dissolve until very high temperatures.

The chart above is for microalloy additions. Vanadium or niobium could pin grain boundaries to even higher temperatures if they were added in greater amounts. But for small additions, titanium works up to the highest temperatures. On the flip side, the titanium carbides form in the liquid during steelmaking and can become very large. The patent says [1] that Ti is restricted to 0.75% to “minimize the formation of primary MX particles.”

Corrosion Resistance

The A-21 patent does not mention carburizing, but the product seems to have evolved in the intended use because the Carpenter website describes it as a “stainless carburizing steel.” Carburizing is the process of adding carbon to the surface of steel by heating it in the presence of a carbon-containing gas like carbon monoxide. That makes the surface harder and more wear resistant. The data sheet even says that A-21 is “the world’s first and only truly stainless carburizing steel” which is an interesting claim. Other stainless steels have been used for carburizing in the past, and the steel is not so unique that other steels could not be used in a similar way. I think what it means is that A-21 is “truly stainless” meaning having improved corrosion resistance compared to prior carburizing alloys. So at some point it seems they determined that A-21 had more potential as a carburizing stainless steel than only using it in the quenched and tempered condition. The data sheet has a picture showing its excellent corrosion resistant compared to high carbon stainless steels:

None of those comparisons are particularly high corrosion resistance steels, but it is still an excellent result. A comparison against Cronidur 30/LC200N would be interesting, for example. The patent mentions Cronidur 30 but I did not see any direct comparisons against its properties other than for hardness. The data sheet says the steel tops out around 36 HRC without carburizing, but with carburizing can be heat treated above 60 HRC. The patent does acknowledge the existence of prior stainless carburizing steels such as Pyrowear 675 and CX13VDW but it says that those grades do not exhibit good corrosion resistance. Those grades are relatively similar to A-21, apart from the use of vanadium rather than titnaium.

What is the chromium content?

You’ll notice that I changed the chromium content of A-21 in this table above to 11 with a question mark, rather than the midpoint of the data sheet which was 12.25%. The reason is because the patents all show “examples” of A-21 which have less than 11% Cr (10.66, 10.83, and 10.86%), and because the patent says the difference between A-21 and those earlier steels is that the earlier ones will form chromium carbides and A-21 doesn’t. The way to do that is to reduce chromium, and CX12VDW already has 12%. So for that reason I believe the actual target chromium content of A-21 is 11% or perhaps even a bit lower. The average of the three “examples” in the A-21 and A-421 patents would be 10.78%, so a target of 10.75 or 10.8% would not be surprising, though when making one-off heats for testing purposes they are not always perfect, and there will always be some variation between a target and the final result.

Molybdenum, Titanium, and Microalloys

The midpoint of the data sheet spec says 0.6% for Mo but all of the patent examples are around 0.5% (0.47, 0.49, and 0.49%). The midpoint for Ti is 0.45% though all of the examples are lower: 0.37, 0.38, and 0.29%. So the target Ti is probably below 0.45%, perhaps 0.35%. Small differences in Ti can mean sizeable differences in the TiC which is why I am nitpicking the Ti amount. The A-21 patent has two examples, one without V or Nb and one with 0.03% V and 0.015% Nb. The A-421 patent lists an example with 0.1% V and 0.06% Nb. So I think they may be making microalloy additions for those two elements.

A-421 and Adding More Carbon

The method for adding more carbon to make A-421 has evolved since the patent to a more conventional method of adding it to the melt.

The patent says [2] that while the steel could be given a carburized surface the design is primarily for having carbon “throughout” the cross section, and adds about knives: “A through-hardened knife blade that utilizes the technology and methods described herein, for example, could be repeatedly sharpened without adverse consequences. This aspect of the invention has been successfully realized with thicknesses of about 0.09 inches to about 0.1 inches. However, it is believed that the invention can be extended to thicknesses up to about 0.125 inches or more.” So it appears that A-421 would be restricted to thinner cross-sections if it was produced with this carburizing manufacturing method.

Originally the patent claimed it was necessary to carburize the sheet to keep the size of the TiC small [2]: “The carbon content of the alloy according to the present invention cannot be obtained conventionally, such as by adding carbon during melting because such an alloying addition would result in a relatively large volume fraction of primary MC particles with a large interparticle spacing…” This is an interesting method and not one I have heard of before, I am only aware of carburizing final parts, not whole steel sheets. It reminds me some of the process Uddeholm uses by nitriding their steel powder to make Vanax or Vancron. But in this case it is the whole steel sheet and not powder.

Interestingly, thermodynamic software does not predict a difference in the TiC formation temperature based on carbon content. This makes some sense; if there is enough carbon to form all of the TiC then the steel will form the same amount of TiC and thus the formation of those carbides should be relatively similar. This is significant because TiC will form at extremely high temperatures where rapid growth is possible. The software predicts a formation temperature around 2770°F. However, it is not totally implausible that producing the steel with lower carbon would lead to smaller carbides. If the thermodynamics of the carbide formation remain unchanged perhaps the “kinetics” (speed of formation) would be.

However, when I spoke to Dr. Buck he told me that the carburization method was not ultimately feasible and that they add the carbon when making the steel instead. I asked about keeping the carbides small and he said that by carefully controlling the composition and using some specific processing they are able to keep the carbide size in check.

The target carbon content is not published in any data sheet or presentation I have found, but ranges are given in the patent. The patent covers a range of 0.2-0.7%, the midpoint of which is 0.45% carbon. Later in the patent it says that hardness greater than 60 HRC can be achieved if the carbon content is between 0.35 and 0.63%, and the midpoint between those is 0.49%, which is why I have assumed the target carbon content is 0.5% for A-421.

Microstructure

There is a micrograph of A-421 which was published in a presentation that has been delivered around to different people but has not been published online by Carpenter. You can see images from it on Spyderco forums.

The micrograph shows relatively small TiC, the largest are somewhere in the range of 1-4 microns, which are the “primary” carbides that form in the liquid steel. There are also many smaller carbides which are the “secondary” carbides that form in the solid steel. And there are even smaller carbides that are only visible with electron microscopy. Technically these carbides could contain some nitrogen, either TiN or Ti(C,N), and also they could contain some niobium or vanadium. So sometimes metallurgists label these as “MX” where M is generic for a metal and X is for carbon or nitrogen. Though I don’t always refer to MX because it is more for metallurgists to be correct than to give real meaning to the person reading it.

I am not sure if this is a micrograph of the earlier carburized A-21 or if this is the final version where carbon was added to the melt. Thermodynamic software predicts about 0.8% MC from the Ti, V, and Nb. As a comparison, here are micrographs of 3V with 4-5% MC and MagnaCut with about 8%. Note that the magnifications are similar but not identical, and also the carbides appear black in the A-421 micrograph and white in the 3V and MagnaCut micrographs.

CPM-3V with about 4-5% MC

MagnaCut with about 8% MC

I am very curious to see more micrographs of the A-421. I have found journal articles [4-5] about steels with similar Ti contents and often the TiC particles are significantly larger than what is shown in the A-421 micrograph. So it would be an accomplishment of its own to be able to maintain the carbide size so small.

Predicting Properties of A-421

So using the information we have about A-421 we can make some predictions about its properties. To summarize what we discussed so far: around 10.8% Cr in solution, can be heat treated to roughly 62 HRC, has no chromium carbides after heat treatment, and has about 0.8% MC which are relatively small. Titanium carbide is high in hardness, even a bit harder than NbC [6]. Those all add up to a steel that should have very good corrosion resistance and toughness with relatively low edge retention. Z-Tuff and CPM-1V also have about 1% MC, though they also have 2-3% chromium or molybdenum carbides. So we would expect A-421 to have edge retention that could be as good as those steels, though probably a bit worse due to having less carbide. Those steels have similar edge retention to AEB-L as well, another comparison point for A-421 in terms of its potential toughness-edge retention balance. We would expect A-421 to have similar properties to LC200N having good corrosion resistance but with somewhat higher potential hardness. Or similar to AEB-L or 14C28N but with improved corrosion resistance. However, LC200N and 14C28N did have somewhat higher edge retention in my CATRA testing than AEB-L, CPM-1V or Z-Tuff (I tested CD#1 which is the same). I wouldn’t expect A-421 to exceed those steels for CATRA testing because of the low carbide content. The Carpenter presentation says “Outstanding edge retention as shown from CATRA testing” but doesn’t give any numbers or direct comparisons.

Fine Blankable?

Many knife steels cannot be “fine blanked” because they have too much carbide and/or are too hard in the annealed condition. Either the equipment does not have the power to blank out the knives or the blanks themselves will fracture during blanking. But fine blanking is important to low cost knives especially. It is a cheaper and faster process than waterjet or laser cutting. 420HC is perhaps the best known steel that is fine blankable, but some knives made with 12C27, 13C26, AEB-L, and 14C28N are fine blanked. One interesting thing I noticed in the A-421 presentation is that it said that it could be fine blanked but it also said the annealed sheet would be 302 BHN max. Of course that is a maximum, but that hardness is quite high for a steel that would be fine blanked. 420HC is reported to be 89 HRB by ATI which would convert to about 188 BHN, much softer than the reported max annealed hardness of A-421. And ATI reports 95 HRB (about 210 BHN) for 440A. For a hardness scale knife enthusiasts might be more familiar with, 302 BHN converts to about 32 HRC, relatively high for annealed hardness. Dr. Buck told me the current product is about 30 HRC in the annealed condition, but they have worked on the annealing procedure in the lab and have gotten as low as 25 HRC. I think that will still be significantly too high for easy blanking.

Conclusions

I like that A-421 is a relatively unique knife steel and that it uses a different composition approach from past steels. If it works out as intended it could offer very good toughness and corrosion resistance in a product being produced in the USA. The remaining questions I have about the steel are whether it can match the edge retention of steels like AEB-L or LC200N and if it falls short by how much. I also have my doubts about whether the steel will be truly fine blankable with the relatively high annealed hardness. And I am also intrigued to see micrographs to see just how small those titanium carbides are.


[1] Buck, Robert. “Fine-grained martensitic stainless steel and method thereof.” U.S. Patent 6,890,393, issued May 10, 2005.

[2] Buck, Robert F. “Strong, Tough, and Hard Stainless Steel and Article Made Therefrom.” U.S. Patent 12,129,536, issued Oct. 29, 2024.

[3] Buck, Robert F. “Creep resistant, precipitation-dispersion-strengthened, martensitic stainless steel and method thereof.” U.S. Patent 5,310,431, issued May 10, 1994.

[4] Kostryzhev, A. G., C. R. Killmore, D. Yu, and Elena V. Pereloma. “Martensitic wear resistant steels alloyed with titanium.” Wear 446 (2020): 203203.

[5] Li, Jing, and Chengbin Shi. Carbide in special steel: formation mechanism and control technology. Springer Nature, 2021.

[6] Bedolla-Jacuinde, Arnoldo. “Microstructure of vanadium-, niobium-and titanium-alloyed high-chromium white cast irons.” International Journal of Cast Metals Research 13, no. 6 (2001): 343-361.

The post Carpenter A-421 Knife Steel appeared first on Knife Steel Nerds.

  •  

How to Heat Treat MagnaMax Steel

Wide Release Date for MagnaMax for Small Knifemakers

MagnaMax will be on sale May 1st, 2026 at 9am on Niagara Specialty Metals’ online store: https://nsm-ny.com/shop/

You can create an account beforehand so that you are ready to buy once the steel goes live. We made the following commercial to get pumped for the release:

Intro

I wrote an article (and created a video) about MagnaMax properties a few months ago. So I won’t be rehashing all of the properties here. Basically, MagnaMax is designed to have enhanced wear resistance and edge retention vs MagnaCut with similar corrosion resistance and hardness potential.

You will also see in the chart above that MagnaMax offers superior toughness and edge retention to the popular M390 and 20CV. It is very difficult to improve both of these properties at the same time, so this is a big improvement. It also maintains similar toughness to grades CPM-154, S35VN, and Vanax, which were formerly the toughest PM stainless steels prior to MagnaCut. So it offers a significant edge retention improvement to those grades, which have had a reputation for good properties in the past.

That property summary article did not have specific heat treatment recommendations because I was waiting on the final material. The initial heat of steel had carbon on the low end of the specification, so it wasn’t as representative of the average material as I wanted. No change was made to the target composition or the specification, it just landed at the lower end for carbon. So now that I have received and tested material closer to the midpoint of the specification I performed a more comprehensive set of tests. Knifemaker Matthew Gregory helped to make the majority of the toughness coupons.

High Level Heat Treatment Summary

Before we get into all of the details I can give a simple summary so you don’t get lost.

With Cryo:

Austenitize 2100-2250°F (1150-1230°C). The baseline temperature for good properties is 2150°F (1175°C).

Plate quench for faster cooling and slightly higher hardness.

After cooling to approximately room temperature, place immediately in liquid nitrogen. The amount of time it sits in the liquid nitrogen doesn’t matter that much, it just needs to reach the temperature. An hour is fine. What does matter is not wasting time before putting it in the liquid nitrogen. You don’t need to check the hardness beforehand.

Temper 300-450°F (150-230°C) twice for two hours each time. 350°F (175°C) is a baseline temperature for good properties.

Without Cryo:

Use your household freezer. It is a myth that it doesn’t have any effect. There is no reason to do no cold treatment. Everybody has or can get a freezer. Dry ice is even better, but despite being about 100°F colder than a freezer often behaves closer to a freezer than to liquid nitrogen.

Austenitize 2050-2100°F (1120-1150°C). 2100°F (1150°C) is a good temperature. It might be possible to go somewhat higher but I worry about excess retained austenite.

Plate quench for faster cooling and slightly higher hardness.

After cooling to approximately room temperature, place immediately in the freezer or dry ice. The amount of time it sits in the freezer doesn’t matter that much, it just needs to reach the temperature. An hour is fine. What does matter is not wasting time before putting it in the freezer. You don’t need to check the hardness beforehand.

Temper 300-450°F (150-230°C) twice for two hours each time. 350°F (175°C) is a baseline temperature for good properties.

Austenitizing hold times:

The required hold time changes with temperature. This is the soak time required after the piece reaches the temperature. It rarely hurts to add extra minutes, it is more common to have an issue with undersoaking.

2050°F (1120°C): 20 minutes

2100°F (1150°C): 15 minutes

2150°F (1175°C): 10 minutes

2200°F (1205°C): 5 minutes

2250°F (1230°C): 5 minutes

Hardness and Cryo

I first made a series of coupons to test the hardening response, including with the addition of a freezer or liquid nitrogen treatment after quenching. I used the soak times in the section above.

You can see that with no cold treatment the peak hardness was 2050°F (1120°C) after tempering at 300°F (150°C). Hardness drops with higher temperatures from excess retained austenite. Hardness rose when using liquid nitrogen all the way to 2250°F (1230°C). It would be unlikely to keep rising much beyond this temperature and the possibility of melting grain boundaries starts to become more of a danger. The freezer also rose all the way up to 2250°F but to a lesser extent. Because the increase was small beyond 2100°F (1150°C) this is why I limited my recommendation for the freezer to that temperature. That makes me think both the retained austenite and hardness of the martensite were increasing beyond that temperature, leading to relatively flat behavior. Excess retained austenite can lead to worse sharpening behavior when deburring. Overall this hardening response is not radically different than MagnaCut.

Nothing too crazy showed up in the tempering. You can see that a cold treatment leads to less hardness loss in tempering. Compare 2050°F with and without a cold treatment, or 2100°F with liquid nitrogen vs the freezer. Note that I have a single curve for both freezer or liquid nitrogen from 2050°F, and this was because the two were sufficiently similar to have a single line. Plus don’t want to make the chart too busy.

You will also notice that the hardness reaches an initial minimum at 600°F (315°C) and then rose to a secondary peak around 900°F (480°C). This is known as “secondary hardening.” I don’t recommend tempering in that range, especially with stainless steels, because it reduces corrosion resistance. For example see two Vanax coupons below, both sprayed with 1% saltwater. The one of the left was tempered at 400°F (200°C) and the one on the right was tempered at 1000°F (540°C).

Toughness

We also tested a series of charpy toughness coupons for this heat of MagnaMax. I used my standard coupon which is quarter size (2.5 x 10 mm) and unnotched. Three coupons were tested for each condition. We used liquid nitrogen in the heat treatment of all of these coupons directly after the quench. We used austenitizing temperatures of 2000-2250°F (1095-1230°C) and tempering temperatures of 300, 350, and 450°F (150, 175, 230°C).

The hardness was slightly lower than the small hardness coupons I showed results from before:

Looking at the resulting toughness, it rose from 2000 to 2050°F (1095 to 1120°C), was relatively flat up to 2200°F (1205°C), and then dropped somewhat up to 2250°F (1230°C). This is why I recommended a baseline austenitizing temperature of 2150°F (1175°C) as this appears to be roughly the peak hardness-toughness, though an argument could also be made for 2200°F (1205°C), in part due to a couple of the 2150°F results being on the low end and a couple of the 2200°F being on the high end. This is likely due to statistical variability of testing.

You can also see that toughness increases with tempering temperature as we would expect, which also corresponds to a hardness decrease. Lower hardness generally correlates with higher toughness.

There was a greater increase in toughness between 300 and 350°F (150-175°C) than between 350 and 450°F (175-230°C), which is why I recommended 350°F (175°C) as the baseline tempering temperature.

Hardness-Toughness Balance

But what we would like to maximize is the highest toughness for a given hardness. So I plotted hardness vs toughness below.

You will notice that the maximum hardness-toughness combinations were generally 2150-2200°F (1175-1230°C) and tempering at 350-450°F (175-230°C). The exceptions include: 1) 2100°F (1150°C) with 450°F (230°C) because that combination gave the best properties for lower hardness. And 2) For maximum hardness you need 2150-2250°F (1175-1230°C) in combination with the minimum tempering temperature of 300°F (150°C). I next overlaid those best heat treatment conditions on top of the similar non-stainless steels K390, Vanadis 8, and CPM-10V:

Erasteel MM#1 is the first heat that was shown in the prior article about MagnaMax properties, and Erasteel MM#2 is the final tested material above. You can see that both have a similar hardness-toughness balance, though the new one is skewed to somewhat higher hardness, as expected from more carbon. You will also see that the toughness is very similar to K390 and Vanadis 8, an excellent result given that MagnaMax is a stainless steel with similar wear resistance. So we greatly improved corrosion resistance over those steels while maintaining their other properties. I next plotted those hardness-toughness values vs other stainless powder metallurgy steels:

You can see that MagnaMax has superior hardness-toughness than virtually all of the powder metallurgy stainless steels apart from MagnaCut. This includes steels with a good reputation for toughness including Vanax, XHP, S35VN, and CPM-154. And below I have the more complete graph of stainless steels which is a bit busy:

Corrosion Resistance

I compared the final higher carbon version of corrosion resistance to the earlier and both passed the 1% saltwater corrosion test. Showing a picture of two clean samples isn’t very interesting, so here is the earlier image of MagnaMax vs other steels:

Each of those was austenitized from 2150°F (1175°C). MagnaMax (and MagnaCut) were designed for all of the chromium carbides to be dissolved around 2050°F (1120°C). After the chromium carbides are dissolved the corrosion resistance doesn’t appreciably change with even higher temperatures. This is different than most other stainless steels which have chromium carbides all the way up to the melting temperature. But using even higher than 2050°F does provide some factor of safety, better ensuring the chromium carbides are fully dissolved.

The other main factors for corrosion resistance are quench rate and tempering temperature. I mentioned in the tempering section that tempering above about 750°F (400°C) leads to a reduction in corrosion resistance and I showed a test with Vanax to illustrate that. Quenching isn’t an issue unless it is very slow, which leads to carbides precipitating on the grain boundaries which can reduce corrosion resistance.

Edge Retention

The primary factors for edge wear resistance are carbide volume, carbide hardness (controlled by type), and steel hardness. While the carbides are very important when comparing different steels, there is less of an impact within a given steel. It is true that austenitizing higher dissolves a bit more carbide but this effect is generally drowned out by the increase in hardness. So in general, achieving a higher hardness results in greater edge retention, and there isn’t much point in worrying about the exact austenitizing and tempering temperatures that were used to get there. I have the graph below of CATRA results I tested previously to show where MagnaMax lands and the effect of hardness on the results:

Summary and Conclusions

So I have shown the majority of the heat treatment data that I generated and my reasoning for the different recommendations. I am overall happy with how the heat treatment response ended up. If you want to see the simplified heat treatment recommendations, scroll back near the top where it said “High Level Heat Treatment Summary.” Hopefully that is simple enough for everyone. If not then ask questions in the comments. MagnaMax will be on sale May 1st, 2026 at 9am on Niagara Specialty Metals’ online store: https://nsm-ny.com/shop/

The post How to Heat Treat MagnaMax Steel appeared first on Knife Steel Nerds.

  •  

Learn from Bad Bark River Design

If you would like to join the Knife Steel Nerds Patreon to support knife research visit Patreon.com/KnifeSteelNerds You can read articles and watch videos early, and at the top level you even get a mug!

I have two classes for “Blade University” at Blade Show Atlanta coming up the beginning of June. They are titled “Factors that Affect Edge Retention” and “What is Coming Next for Knife Steel?” Read more and buy tickets here: https://bladeshow.com/show-info/classes/

YouTube Video

Bark River Closing Down

American company Bark River Knives is shutting down. There is a pretty good write-up of the situation in this Outdoor Life article. One thing the article doesn’t discuss is the large number of people coming out now who say that Bark River or Mike Stewart owes them money for past services or products. Since the company is going away, I thought this was a good opportunity to discuss the mistakes it made in design and manufacturing that others can learn from. This includes other knife manufacturers and custom knifemakers. And for knife buyers, you can look for signs that indicate issues with a knife before purchasing it.

Mislabeling of Steel

One of the biggest controversies of the Bark River situation is the owner, Mike Stewart, admitting that they were purchasing China-produced blanks, reworking them, and stamping CPM-154 and “Made in USA” on them. He also defended this practice saying in their testing the steel was almost as good as CPM-154 and that since they performed “5 operations” on each knife that counted as Made in USA. Testing a steel and saying it is “almost the same” does not mean you can mislabel it. I think that much is basic. You can’t buy a car manufactured in China and decide it works just as well as a Dodge Charger and slap the logo on it. This would be illegal for infringing a trademark, both for the Dodge Charger and for the CPM-154. Also, Mike Stewart seems to have a very poor understanding of what “Made in USA” entails. Even if he had started with raw barstock from China and manufactured the knife from start to finish it would still not be legal to mark it as “Made in USA.” He would have to have a qualified label like “Made in USA from imported materials” or something along those lines. But even that label would of course not qualify when starting with a finished knife blank from China. But as a steel metallurgist, the most upsetting part to me is the misrepresentation of what the steel is. It’s obvious they just don’t care what the steel is as long as they can justify putting a label on it they think would sell better.

Broken Bark River Scout Knife

In 2022 there was a video from Dutch Bushcraft Knives (DBK) where they tested a knife in MagnaCut from Bark River Scout and it broke at the jimping while they were batoning (autocorrect does not like either of those words).

  

They talked to Bark River and were told the fault was with the steel and they pointed out some discoloration in the fracture surface, claiming this indicated an inclusion in the steel. An inclusion is a non-metallic compound in steel like an oxide or sulfide. Inclusions are present in every piece of steel, the question is about how many and how big. Inclusions that are so large you can see them with the naked eye are rare, and the discoloration they pointed out in the video does not look consistent with an inclusion.

Another Broken Bark River Scout

Bark River broke a knife of the same model in MagnaCut during manufacturing and sent it to Niagara Specialty Metals requesting an investigation into the steel. Bob Shabala of Niagara sent the blade to an independent third-party metallurgist named Gary Maddock. He evaluated the broken blade and sent a report to Niagara and Bark River.

Stress Concentrations

So this is a completely different knife of the same model that broke in the same exact place. And not even from using the knife but just while manufacturing it. So we must start discussing what a “stress concentration” is (also called a “stress riser”). I wrote a whole article about stress concentrations back in 2019. As the name implies, a stress concentration is any region of a part where the stress is concentrated. One simple way of concentrating stress is by having a reduced area in a portion of a part. As a metallurgist we often perform “tensile tests” where the standard is to have a reduced cross-section in the region to be tested. This ensures (almost 100%) that the fracture will occur in that reduced area:

Stress is just load divided by area, so if the width in that region is half of the rest of the flat piece, the stress would be twice as much in that region. However, stress concentrations can be much more extreme than this. The most common example of a bad stress riser is a sharp corner. This leads to very high stress in a small region of a part, such as is shown in this simulation:

The red region shows a much higher stress than the rest of the part being pulled apart. So we can predict with some high level of certainty that this part would break right at those sharp corners. This is all relevant, of course, because the jimping on that knife led to a stress concentration when the knife is being flexed.

So how could Bark River have avoided the stress concentration of the jimping? One method is to remove the jimping altogether, of course. There has been debate in the knife community for decades as to whether jimping is beneficial. Another way would be to round out the design of the jimping to reduce the stress concentration. Making it shallower and more rounded would be beneficial. An example would be this FreeReign knife from Demko:

Surface Roughness

Another important factor in this knife breaking is that the method used to cut the blank led to a very rough surface, and that surface was not cleaned up within the jimping.

So Gary Maddock noted that the rough surface in that jimping may have accentuated the stress riser. The rough surface has many discontinuities in it; basically areas that already look like a crack. It makes crack initiation easier because a crack is already half formed. The other thing he noted is that there was “No evidence of thermal damage” and “Microstructure appears normal under the surface.” He noted this because laser cutting can lead to a “heat affect zone” (HAZ) where the microstructure can be different than the rest of the steel. Laser cutting essentially means the steel is being locally melted, so when steel has been melted and resolidified this leads to a cast structure which is likely to be more brittle than the rest. Even away from the melted region the steel can be rehardened and thus be harder and more brittle than the bulk steel. So for both the possibility of HAZ with laser cutting and for high surface roughness with laser or waterjet it is best to refinish the perimeter of blades after they are cut out.

Bark River MagnaCut Corrosion Resistance

Some Bark River Knives were reported to easily stain or rust in MagnaCut. Mike Stewart claimed that was because MagnaCut is not a stainless steel. He claimed “i would never have listed this as a True Stainless – Crucible does but I disagree with them.”

It is silly that he was claiming to have knowledge of what classifies a steel as stainless better than the steel manufacturer itself. The most basic definition of what a stainless steel is is that it has at least 10.5% Cr, which MagnaCut has. However, this definition is overly simplistic, as there are some steels like D2 tool steel which are famously not stainless despite having enough chromium to meet that definition. The high carbon (and lack of most other elements) in D2 means that about half of its chromium is tied up in carbides and thus cannot contribute to corrosion resistance. The stain resistance from chromium comes from the element forming a chromium oxide layer at the surface. If the chromium has already formed a compound with the carbon it is not able to form a compound with oxygen. This available chromium is known as chromium “in solution” in the iron. As I have covered in the article about MagnaCut development, it was designed to not have any chromium carbide in the microstructure after heat treatment. As another side note, while the bulk chromium of MagnaCut is 10.7%, because the steel is about 8% vanadium/niobium carbide (leaving 92% steel matrix), the chromium in solution is actually higher than 10.7%, closer to 11%. This is because very little chromium is present in the vanadium and niobium carbides. In other words, if there was no chromium in those carbides the chromium in solution would be 10.7 divided by the volume of the steel matrix, 0.92 = 11.63%. And the true test of corrosion resistance is in actual corrosion testing, where MagnaCut does very well compared with other stainless knife steels.

Heat Treatment

I talked to people with some knowledge of Bark River heat treating and I did not uncover any practices that would lead to poor corrosion resistance on that side. As far as I know Bark River only sends knives to outside heat treating companies, and what information I could obtain indicated they did not request any modifications to the heat treatment.

Belt Contamination?

Another theory I have seen commonly is that Bark River is using the same belts on MagnaCut that they used on non-stainless steels, leading to easily rustable particles on the steel. Bark River vehemently denies this, claiming that they do not mix the belts. This could be true but particles left of the steel could still pose an issue. For example, they might not be thinking of certain polishing steps they are performing where it is unlikely they are swapping anything out – such as buffing wheels. However, one thing to note is that particles left on steel, even stainless steel particles left on itself, can still promote corrosion. These particles are very small and very high surface area, and they act as sites for corrosion to initiate. There is a standard industry practice called acid passivation where stainless steel is treated with a weak acid, typically nitric or citric acid, which is for the purpose of removing free iron from the surface. These practices are not that common in the knife industry as far as I have seen but it is still a good example of how the condition of the surface is very important for future corrosion resistance. There are many other factors that a corrosion expert would want to discuss such as surface finish (finer is better), whether the steel is in contact with any other metals such as pins or bolts, etc.

Do We Know Why?

I cannot say definitively why Bark River knives have had reports of poor corrosion resistance with MagnaCut. The above is only laying out some of the possibilities.

Did Bark River Actually Use MagnaCut?

There is a video from Gravy Train Outdoors where he claims to have XRF tests that show Bark River MagnaCut knives were not actually made with MagnaCut. XRF testing is common for confirming the composition of steel when someone is concerned it has been mixed up. These testers are often called “Positive Metal Identification” (PMI) testers. However, I reviewed this video and found many problems with this testing:

  1. He says in the video that this is a soil XRF tester, not one designed for distinguishing metals.
  2. He reports a composition in an AI readout he used to interpret the results, but also shows the readout from the tester at the end. They do not look even remotely similar to each other. For example, he makes a big deal of a significant amount of tungsten (1.3%), which is not an intentional addition to MagnaCut. However, at the end when he shows the tester its screen reports that tungsten was not detected. I don’t know if the data file he got to feed into the AI was not from his tests, or if the AI misread the file or hallucinated its own values.
  3. The composition he reports in the video, and those visible on the tester at the end – do not look like any known steel. I actually have no idea how to read the results of the tester since it says 160% iron. Perhaps that has something to do with it being a soil tester.
  4. He showed in the video another MagnaCut Buck knife but it was not tested with the soil tester. He would likely have seen that its results also do not make sense with the soil tester.

The report from Gary Maddock did not include a composition measurement but the microstructure does look like MagnaCut. Niagara Specialty Metals reported that they checked it with XRF before sending it to Maddock but did not formally record the result.

KnivesShipFree has had some independent XRF testing performed and not found any knives to be mislabeled in their inventory apart from the Chinese mislabeled CPM-154.

DLT has shipped knives to Niagara Specialty Metals to check their knives with XRF.

While I can’t rule out the possibility of there being mislabeled MagnaCut knives from Bark River, I have not seen any evidence to suggest that there are.

Conclusions

Stress concentrations are quite common in knives, both production and custom. It seems to be an element that is rarely considered by designers and makers. If you want a high-performing knife that won’t break, they need to be considered in the design process and when purchasing a knife. For knife manufacturers and knifemakers it also helps to test a knife in ways that are at the extremes of their intended use case. This type of testing would have quickly shown Bark River that their knife was not ready to handle any task with small flexing forces.

The post Learn from Bad Bark River Design appeared first on Knife Steel Nerds.

  •  

3 Times Knifemakers Proved Metallurgists Wrong

If you would like to support knife steel research, join us at Patreon.com/KnifeSteelNerds. You can read articles and see videos early, discuss topics with fellow steel nerds, and even get a free Knife Steel Nerds mug!

Video

There is also a video version of the following article:

Metallurgists and Knifemakers

Back in 2022, I did a YouTube video called “Do Knifemakers Know How to Heat Treat?” I found video clips where knifemakers explained how to heat treat and how it works, and then I pointed out the misconceptions and misunderstandings they had about metallurgy and heat treating. It worked well because responding to how the knifemakers explained things let me address commonly repeated, untrue claims. Because when I cover my own material, I’m typically just teaching, rather than correcting misunderstandings. However, a handful of comments on the video said I was being unfair or unkind to the knifemakers.

I was a bit surprised by those comments because I thought, “Of course I know more about how steel works because I am a professional PhD metallurgist, so no one should be offended about teaching my discipline.” However, we can always debate the proper tone for such things. But I also think some people misinterpreted my mindset in the video as criticizing, or even parodying, the knifemakers’ understanding of metallurgy. There are also some knife buyers (and even fellow knifemakers) who will lionize the heat-treating prowess of certain knifemakers and believe that they know more than they do. The level of metallurgical understanding of knifemakers varies widely, from knowing almost nothing to having a professional level of knowledge. Many knifemakers are curious about metallurgy because they want to make the best possible products.

Blade Cutlery Hall of Fame Dad and Me

This is largely why I became a metallurgist. My dad, in his knifemaking and Damascus-making, loved learning about metallurgy, and I wanted to learn about it as well. (You can watch an interview with him here). Growing up, my father and I were always excited about the prospect of speaking with metallurgists, such as employees at Crucible Steel or Professors like John Verhoeven. Hoping to gain some secret knowledge from these professionals who had dedicated decades to studying steel. Even now that I am a metallurgist, there is still much to learn. I often learn new things from blacksmiths, bladesmiths, and knifemakers. They may have practical experience that contributes to my understanding of steel. So this article is dedicated to the times when craftsmen taught metallurgists things.

“Damned Good Stuff” and Impact Testing

Harry Brearley invented stainless steel in the early 20th century (1912-1914ish), and he developed the common 420 stainless steel, which remains widely used in knives. I wrote a whole chapter in my book, The Story of Knife Steel, about him and what led to the discovery of stainless steel. I pulled a lot of quotes from him because I thought he was funny and interesting.

Brearley credited cutlery manager Ernest Stuart of Mosley Cutlery Company with the success of stainless steel [1]: “It is due to him to say that, from the very first trials, he had confidence in the possibilities of the steel. He made unremitting efforts to adapt the process of knife-making to the unusual qualities of the steel and, so far as the initial use of stainless steel for cutlery is concerned, the credit is due to him and his firm.” Stuart was also the one who named it “stainless” steel, giving it the name it still has today.

The reason I bring up Brearley is because of things he wrote about working with practical craftsmen (such as Ernest Stuart) and their contributions to the understanding of metallurgy. His father was a steelworker and had no scientific training. Brearley said that he was “in appreciation of men, typified by my father, who have exerted a greater favourable influence on the practice of steel-making than they are given credit for.”[1] “The value of scientific control, with its measurings and weighings, is undeniable, but it is sadly blemished by a strutting vanity and snobbish intellectual pride which smothers with confusions aspects of a subject it does not understand.”[1]

Brearley also said that his brother was a more hands-on person than he was [1]: “He is a better workman, a better observer and more resourceful experimentalist than I am; but he has stuck to the furnaces, mills and forges and done things whilst I have read about them, and looked at things other people were doing, and taken some trouble to describe them in the language learned from books.”

Caption from Brearley: “My brother (sees) more with the naked eye than most people see in them using laboratory equipment. On the other hand, I spent about 20 years in a laboratory, mainly occupied in measuring things. The picture is intended to be symbolic: My brother on the right-hand side is looking at a fractured surface of a piece of an ingot, and I on the left-hand side am pretending to be doing something with a pair of calipers.”

To illustrate the fact that ordinary workers often have methods that are superior to the scientist, Brearley described the history of toughness testing [1]:

For a century or two the blacksmith has been in the habit of ending a bar of iron or steel after first nicking it with a slate. When the bar is broken, as intended, through the nick, the effort required to break it, appreciated by the smith’s muscles, is registered in his mind – his extremes of judgement are “rotten” and “damned good stuff.” There is not the slightest doubt in the smith’s mind that the material he intends to make something from is all the worse for being “rotten” and all the better for being “D.G.S.” Many years ago, thirty maybe, a young man in Rugby, named Izod, was called upon to explain why of two pieces of steel one failed hopelessly and the other did its job very well. Both chemical analysis and every conventional form of mechanical testing showed that the two pieces were identical; but this young man knew they were not. Bethinking himself of the blacksmith, he notched both pieces, and found the one was “rotten” and the other “D.G.S.” In order to state the difference, which was the only difference he could find, quantitatively, he made a pendulum hammer very much like the existing Izod testing machine, and then went to South Africa, blissfully unconscious that his Rugby adventure was the lead to a new kind of official testing.

This is a good example of a time when blacksmiths had a simple test for telling whether a piece of steel was processed correctly, and the methods used by the metallurgists would not reveal these most basic properties. The common test used back then by metallurgists, which continues to this day, is the tensile test. The tensile test involves pulling a piece of steel (tension/tensile) until it breaks. The load capacity of the steel is measured during this test along with how much the steel has elongated while it is tested. This generates a “tensile curve” that shows the yield strength, ultimate strength, and ductility (amount of elongation) of the steel. So there is a lot of information that is gained in one simple test.

You’ll see the different regions of a tensile test above. The “elastic deformation” region is where if you remove the load the piece of steel returns to its original dimensions. This is like bending a paper clip and letting go, it returns to the original shape. You will notice that the “curve” is in fact a straight line in the elastic region; as you load the steel it gets longer, and if you let go it returns to its original length. However, if the “yield point” is exceeded, the steel will remain permanently elongated. Just like if you bend a paper clip too far it will remain bent. The “ultimate strength” is the maximum stress the steel can take (stress is load divided by cross-section). The stress actually drops after that until the steel breaks while the steel “necks,” the steel reduces its cross-section before fracture.

In Edwin Izod’s recounting of his learning about impact testing he said [2]:

For some considerable time, however, owing probably to the greater facilities now available, tensile tests … seem to have displaced almost every other test, and in many present-day specifications for steel no other test is prescribed. In special cases, however … it is usual to include a falling-weight test. … [O]bviously a steel that possesses inability to withstand shock would be immediately detected by this method, and it is highly probable that many cases of peculiar breakage would have been avoided had a standard brittleness test been specified, as well as a tensile test; in fact, fractures have occurred in steel which are inexplicable by known chemical or standard physical tests; and some experiments … show that a ductile steel, as evidenced by the usual tensile tests, may be exceedingly brittle.

So he found that a rapid impact test behaved differently a tensile test. This became known as the Izod impact test, which is similar to the Charpy impact test. The difference between an impact test and a tensile test is in the “strain rate” of the test. Tensile tests are done with a relatively slow increase in load being applied. If you take a knife edge and flex it, or take a whole knife and bend it, you are performing an operation relatively similar to a tensile test (or a bend test), where the load/stress is applied fairly slowly. However, if the steel is rapidly impacted the behavior is somewhat different. This is like chopping something hard with a knife, or dropping a knife tip-first into the ground. The knife may have been fine with cutting hard materials, but when dropped the tip broke off. The rapid rate of an impact test can induce brittle behavior in otherwise ductile materials. Blacksmiths had already known this from their experience with breaking pieces of steel, but it took metallurgists longer to figure that out.

Schematic diagram of Charpy impact test

Tensile tests also reveal brittle materials (see below), which shows up with a low ductility result. In fact the majority of knife steels are very high in hardness and contain brittle carbides, so most of them do not have much ductility in a tensile test. Bending tests tend to do better with tool steels because the tested volume is smaller. However, there are certain types of embrittlement that do not show up in a tensile or bending test and are better revealed through impact testing because of the strain rate difference.

Example tensile curves from here

Frank J. Richtig

I previously wrote about Richtig in an article about his knives. I also covered his history in The Story of Knife Steel book. Richtig began as a blacksmith apprentice at 19 years old in 1906. In 1908 he and a friend set up their own blacksmithing shop until 1923, when he sold his share. In about 1916, he began experimenting with a heat treating process for knives. In July 1925, he leased a shop and began producing knives. Despite his previous experience as a blacksmith, his knives were made by stock removal. His typical knives had a cast aluminum handle though some rare knives had leather washer handles. He primarily produced kitchen and butcher knives though also produced some fighting knives for soldiers.

A Richtig butcher knife that I own

In the early 1930s, Richtig and his wife began traveling to the state fair to demonstrate the superiority of his knives. They would take old pieces of steel like railroad spikes, axles, or horseshoes, and he would hammer the knife through the steel and then slice through newspaper afterward. In 1936 his knives were featured in Ripley’s Believe It or Not!, which was published in newspapers across the country. Richtig advertised that his knives could pass these tests due to superior heat treating [3] : “We have discovered and developed a special new process in tempering knives. This method of tempering assures you of a better and more lasting quality of cutlery.”

Richtig in Ripley’s Believe it or Not

Richtig did, however, say that hammering his knives through iron or steel would void the warranty, and that the knives were ground somewhat thicker for the demonstrations [4]:

If knife proves to be defective in any way within six months after purchase, return same to us and we will gladly replace it. However, if the knife blade back shows it has been hammered upon or shows abuse in anyway, the guarantee is void and the knife will not be replaced… These knives are made of high-grade steel and are suitable for all ordinary uses in the home or place of business. They will do all we claim for them. In reference to the cutting of cold chisels, axles and many other steel articles, I wish to say that in my steel and iron-cutting demonstrations, I use the same steel and temper you will find in my regular stock knives. The size and thickness of the blade is the same, the only difference you will find is in the grinding of the cutting edge. I do not sell my knives for the purpose of cutting steel and iron. The purpose of my steel-cutting demonstrations is to show the toughness and temper in my knives. Many thousands of people have seen my steel-cutting demonstration and were greatly amused by them. Striking a knife with a heavy hammer in cutting steel requires special skill and experience, both of which I have learned and mastered during the thirty years I have been making and improving these knives. My knives are made for general all-around use where good, substantial knives are required.

Richtig’s impressive feats have led many to try to find his heat treatment process. Measurements of Richtig’s knives revealed that the steel composition was nothing special, a simple high-carbon steel like 1095 or W1 [5] . Richtig used steel from the Ryerson Steel Company in Chicago, branded as Ryolite [6] .

When Glen Lambert asked him about his heat treating process, Richtig answered [7], “A man is entitled to some secrets, and that’s mine.” He told Lambert [7] “he had found no one worthy of being told or taught his knifemaking, and until he did, nobody was going to get his ‘secret.’ During his declining years no one came forward, and when he passed away … so did the tempering process.”  Of course, this didn’t stop people from trying to recreate his heat treatment. His legend only grew in recent decades as two research papers were published in 2000 [5] and 2015 [8]. The 2000 paper proposed that Richtig had been using an “austempering” process for a bainite microstructure, a type of heat treatment that wasn’t discovered until after Richtig was already famous for his knives’ superior heat treatment. Read about austempering and bainite in this article. In the research reported in 2015, they heat treated 1095 steel using an austempering process and could not match the superior properties reported in the 2000 research paper!

However, there are problems with this conclusion. One is that the hardness of Richtig’s knives varied widely; the knife the researchers attempted to mimic was only 39 Rc, while another knife they tested averaged 50 Rc. The butcher knife I purchased measures 57 Rc. Harlan “Sid” Suedmeier has also tested several Richtig knives and found them to vary in hardness. While Richtig owned a Paragon electric furnace for heat treating, Suedmeier is not sure when he obtained it, which could explain some of the variability. Paragon furnaces did not start until 1948, though perhaps he had another furnace before then.

The two knives analyzed in the 2000 paper

The very low-hardness knife from the research paper is thicker than many of his other blades, and the microstructure shows evidence that the knife wasn’t fully hardened. This “intermediate” microstructure is challenging to mimic with a typical oil quench and temper, or even austempering treatment. The soft phases are very ductile and give the overall steel greater ductility. So the blade that was used for the tensile testing was likely softer than the majority of Richtig knives and was not representative of the typical properties.

The large knife was only 39 Rc and was not fully hardened as can be seen by the remaining pearlite and ferrite

The small knife was fully hardened

Another issue in the 2015 paper where they tried to mimic the 39 Rc knife was that they used a test specimen size that was much larger than what was used when generating the strength-ductility values in the original 2000 paper. The use of a larger test specimen leads to the same strength value but a significantly lower ductility value. One of the researchers from the 2015 paper, Dr. Jared Teague, has since commented that he believes the specimen size is likely the cause of the lower ductility values in that study.

Comparison of tensile curves from a small tensile specimen (red) and a standard tensile specimen (blue). The small tensile specimen had the same strength but measured much greater ductility.

When comparing the tensile properties of the soft Richtig knife to quenched and tempered 52100 in the 2000 paper, they found that the soft steel had better ductility (strain) for a given level of strength (blue dots). Another evidence of the underhardened nature of the soft Richtig knife is comparing the yield strength (red dots) where you can see that the Richtig knife yielded at a much lower stress.

And while the researchers from the two papers were impressed by the properties of the underhardened steel from Richtig’s large knife, in their testing they even found that 52100 austempered at 300°C (570°F) had superior strength (blue dots) and ductility (green dots). However, the 400°C austempered condition was similar to the Richtig knife for strength and ductility. However, the yield strength was higher for the researchers 400°C austempered condition. This shows that it is unlikely that Richtig was using austempering for bainite.

So how did Richtig accomplish his steel-cutting feats? He gave us the clues in the information he had previously provided: he left the edge thicker, and he had 30 years of experience cutting iron and steel with them. Sid Suedmeier, an expert on Richtig knives, shared similar thoughts. I asked him what Richtig’s secret was, and he gave me a one-word answer: “Practice” [9]. The steel and heat treating that Richtig used were not necessarily extraordinary, but he made good knives and was not afraid to test them. His showmanship in demonstrating his knives gave the buying public an irresistible hook, and he became famous for it. But I think Richtig’s most impressive feat might be bamboozling metallurgists several decades later into believing he was using a super heat treatment.

Questek Ferrium M60S Steel

M60S was a brand new steel designed specifically for knives and cutlery that was announced back in 2003. I have written about this steel previously in this article, where I more thoroughly described its history and the design behind it. Here is the first page of the datasheet which advertises what was supposed to make it better:

Questek is a company that designs new materials using “Integrated Computational Materials Engineering” (ICME). In other words, they use computer simulations to design new materials. This sounded especially forward-thinking and advanced in 2003. A new knife steel designed by computer-aided metallurgists? Wow! However, this steel never came to market. I contacted the inventors of this steel about why it didn’t come to market and Professor Greg Olson told me by email: “I recall denting of cutting edges due to early yielding from retained austenite.” I had remembered this result. Knifemaker Jerry Hossom reported edges that deformed easily from a sample of the grade he had been provided, heat treated to 60 HRC [10]. Hossom also reported that a knife in S30V had very little damage [11].

Jerry Hossom test of chopping an 8d nail. 61 HRC 154CM (top) and 60 HRC M60S (bottom).

What led to the easy deformation? It wasn’t hardness, 60 HRC was roughly the same as the 61 HRC of the 154CM blade. The difference was in the yield strength of the material. Typically yield strength and hardness are highly correlated, but there are some cases where they deviate. If you look at the M60S datasheet you will see that it says at 60 HRC the yield strength was 250 ksi and the ultimate strength was 350 ksi. This is a relatively low “yield ratio,” or the ratio of yield strength to ultimate strength, YS/UTS. This means that in terms of yielding behavior, the stress required to deform this steel would be lower than other steels heat treated to 60 HRC. I have seen some people speculate that this lower yield strength comes from the strength of this steel being achieved with carbide precipitation rather than strictly higher carbon martensite. However, when comparing the yield strength of Ferrium-series steels [12] to AerMet-series steels [13-16], a non-stainless precipitation strengthened steel, the Ferrium yield strength is significantly lower (M60S is the orange dot):

You can see that as the ultimate strength increases, the yield strength of the two sets of materials diverges more and more. This is somewhat clearer if we plot vs yield ratio instead:

You can see that for the AerMet grades the yield ratio was flat with increasing ultimate strength (and hardness), but for the Ferrium grades like M60S the yield ratio decreased. So while a lower hardness/strength Ferrium grade has been commercialized as Ferrium S53, the yield strength issue became more relevant after pushing the hardness up to 60+ HRC for knives. As Professor Olson noted, this was due to excessive retained austenite in the higher strength Ferrium grade M60S. When steel is quenched from high temperature it transforms from the austenite phase to the hard martensite phase. With certain compositions and temperatures, the austenite does not fully convert, leading to “retained” austenite. Retained austenite can lead to reduced yield strength even while at the same hardness:

Caldie data from [17]

Data from [18]

The Ferrium grades may be more prone to having excess retained austenite than AerMet due to the high chromium content required for being a stainless. It might be possible to modify the alloy design to overcome this limitation but it probably wasn’t worth the time and expense required for doing so. But this is yet another case where a practical test by a craftsman revealed an issue that metallurgists did not predict beforehand. In Professor Olson’s email to me he had also noted that Al Pendray had made a knife in the steel, which I have included a picture of below.

Al Pendray knife in Ferrium M60S

Metallurgists and Knifemakers Working Together

Of course for many of the examples above, the knifemakers/craftsmen and metallurgists were not antagonistic towards each other. Some of the best breakthroughs happen when they work together on a common goal. One of my favorite examples is bladesmith Al Pendray and metallurgist John Verhoeven.

Al Pendray was a bladesmith trying to develop a consistent process for making Wootz. Verhoeven is an emeritus metallurgy professor. Both men reported that they needed the other to solve the question of how Wootz Damascus was made. I won’t recount the entire history here. Verhoeven has a book about the history which I reviewed here. And I also have a chapter about it in The Story of Knife Steel. There are also a couple of videos on YouTube (Video 1 and Video 2). But I will include a couple of my favorite quotes about what the two thought of each other.

Pendray Wootz knife

Verhoeven said about Pendray [19]: “He could have gone to college and gotten a Ph.D. just like that. I never worked with anybody that could learn faster. And he is extremely patient. I think Al is an amazing man. It’s been a pleasure for me to know him.” Verhoeven also reported that Pendray said that it was another famous metallurgist who encouraged him to pursue the mysteries of Wootz [20]: “Al often spoke in a sort of reverent tone of ‘Dr. Cyril Stanley’ and how Dr. Smith had taken him aside at the meeting, encouraged him in his work, saying that it was his opinion that the mystery of how to make these blades would probably be solved by a working smith.”

My Own Experiences

I did a really big study on pattern-welded Damascus a few years ago. My father was a major supporting person in this study as he produced quite a bit of the Damascus for the study. One of the combinations he wanted to look at was 1095 and nickel. The nickel is very soft while the 1095 was heat treated to high hardness like normal for a knife. He felt this might be a good combination to determine if the “Damascus cutting effect” could happen, an old claim that a combination of hard and soft metals could lead to a saw-tooth or serration effect leading to higher slicing edge retention. I told him we shouldn’t waste our time because it wouldn’t work but he insisted. When we tested it we found – it out-cut plain 1095 by a significant margin, out-cutting every other low alloy steel combination, even ApexUltra/L6. In other words, we proved the Damascus cutting effect. And while we didn’t find that effect for several other combinations, it took my knifemaker father to convince me to look at it in the first place.

I hope you enjoyed being tricked into learning about tensile tests in these stories of metallurgists and craftsmen.


[1] Brearley, Harry. Steel-Makers and Knotted String. Maney Pub, 1995.

[2] https://archive.org/details/sim_engineering_july-december-1903_76/page/431/mode/1up

[3] https://history.nebraska.gov/blog/stronger-steel

[4] Suedmeier, Harlan. “More About Richtig Knives.” Knives ’88. 1987.

[5] Wadsworth, Jeffrey, and Donald R. Lesuer. “The knives of Frank J. Richtig as featured in Ripley’s Believe It or Not!®.” Materials characterization 45, no. 4-5, 2000: 315-326.

[6] Suedmeier, Harlan. Phone conversation, 2022.

[7] Lambert, Glen. “F.J. Richtig: Believe It or Not Cutler.” Knives ’84. 1983.

[8] Teague, J., R. LeMaster, J. Rinksc, A. Winkelmannd, and L. Bartlett. “Attempted Replication of Frank Richtig’s Forgotten Steel Heat Treatments.”

[9] Suedmeier, Harlan. Phone Interview, 2019.

[10] https://www.bladeforums.com/threads/3v-why-arent-more-companies-using-it.407739/post-3800523

[11] https://www.bladeforums.com/threads/s30v.485714/page-2#post-4754204

[12] Kuehmann, Charles J., Gregory B. Olson, and Herng-Jeng Jou. “Nanocarbide precipitation strengthened ultrahigh-strength, corrosion resistant, structural steels.” U.S. Patent 7,967,927, issued June 28, 2011.

13] https://www.carpentertechnology.com/hubfs/7407324/Material%20Saftey%20Data%20Sheets/AerMet%20340.pdf

[14] https://www.carpentertechnology.com/hubfs/Data%20Sheets/AerMet100.pdf

[15] https://www.carpentertechnology.com/hubfs/Data%20Sheets/AerMet_360_Datasheet.pdf

[16] https://www.carpentertechnology.com/hubfs/Data%20Sheets/AerMet%20310.pdf

[17] Rehan, Muhammad Arbab, Anna Medvedeva, Berne Högman, Lars‐Erik Svensson, and Leif Karlsson. “Effect of Austenitization and Tempering on the Microstructure and Mechanical Properties of a 5 wt% Cr Cold Work Tool Steel.” steel research international 87, no. 12 (2016): 1609-1618.

[18] Park, W., M. R. Hilton, A. R. Leveille, and P. C. Ward. “Microstructure, fatigue life and load capacity of PM tool steel REX20 for bearing applications.” Tribology & Lubrication Technology 55, no. 6 (1999): 20.

[19] Oppenhemier, Todd. Alfred Pendray, Wootz Hunter – An Homage to a Remarkable Craftsman. YouTube video, 2018.

[20] Verhoeven, J.D. Damascus Steel Swords: Solving the Mystery of How to Make Them. 2018.

The post 3 Times Knifemakers Proved Metallurgists Wrong appeared first on Knife Steel Nerds.

  •  

Testing Erasteel MagnaCut (vs Crucible Original)

Crucible, Niagara, Erasteel, and MagnaCut

In case you haven’t been following steel news, Crucible Steel went through a bankruptcy and no longer exists. I interviewed Bob Shabala of Niagara Specialty Metals about this transition several months ago. Niagara is the company that purchased ingots from Crucible and would hot roll, anneal, and distribute them to knife companies and steel suppliers. They have also recently started a new online store to better sell directly to individual knifemakers. Niagara has managed to keep production going for a wide range of Crucible (and other) knife steels, including:

MagnaCut, CPM154, S30V, S35VN, S45VN, S90V, 3V, 4V, CruWear (NSM Wear), 154CM, 20CV, M4, CPM D2, D2, 440C ESR, 416SS, 6-4 Titanium. MagnaMax should be available in early 2026.

Erasteel purchased the rights to Crucible Steel trademarks. Erasteel is headquartered in France, but its powder metallurgy production is in Sweden. Niagara worked with Erasteel to retain the exclusive rights to purchase MagnaCut ingots and sell the steel to knifemakers and knife companies. Erasteel produces very high-quality powder metallurgy steel. Bob Skibitski was the head of the powder metallurgy steel production at Crucible Steel for 20 years and was hired by Erasteel. He reports that Erasteel production yields higher-quality, “cleaner” steel. You can read his thoughts in an article on Niagara’s website.

Video

There is a video version of this article:

Previous Testing of European Powder Metallurgy Steels

I have published two studies before comparing manufacturing from different powder metallurgy companies. One compared M390, 20CV, and 204P (with the somewhat different Elmax thrown in). The other compared Z-Wear (same as CPM-CruWear) between Crucible and European production. With the M390/20CV/204P study I found the biggest difference between manufacturers was the oxygen content. Oxygen is an impurity and it leads to oxide inclusions that are detrimental to properties. This is something advertised by companies like Bohler-Uddeholm, that their process is “cleaner” and leads to fewer oxides. However, the toughness of the grades was identical, perhaps in part because the carbide content is quite high and carbide size of M390/20CV/204P are basically the same. Even though Bohler advertises a finer powder size, the carbide size is mostly a result of carbide “coarsening” during high-temperature processing after the powder is made, rather than differences in powder size.

M390

20CV

So the carbide volume, carbide size, and resulting toughness are primarily controlled by the composition and method of manufacture (powder metallurgy) rather than the quality of the production. If the oxides are smaller and in a lower volume than the carbides, then the limiting factor for toughness is the carbide, and so oxide inclusion content doesn’t much come into play.

In the Z-Wear study I thought there might be more of an effect of oxide inclusions than the M390 because it has significantly lower amount of carbide. However, the two steels tested relatively similarly in terms of toughness:

In this case the European-produced version of Z-Wear had slightly higher toughness but it was also at a lower hardness, giving it a slightly worse hardness-toughness balance. In general I called them equivalent in the article. I actually suspect that Zapp had accidentally mixed up the labels of the steels because the oxygen content was lower in the steel that was labeled as “USA” once it was delivered to me. That would mean the European steel had a slightly better hardness-toughness balance, rather than the USA Crucible version.

USA vs European Z-Wear that might have been mislabeled before they were sent to me

Dialing in the Composition for Erasteel MagnaCut

With switching over to Erasteel for MagnaCut production we had several things we needed to figure out. One that might be surprising to people is that steel composition testing is highly dependent on calibration of the instrument and which technique is used. For example, there were significant differences in composition measured between grades in the M390/20CV/204P study and the Z-Wear study. This is not always clear because there is some distribution of composition in manufacturing. If the target is 10% chromium, there is some acceptable range by the manufacturer like 9.5-10.5% Cr. So you can’t measure just one example from different manufacturers and know what the offsets are. So we took pieces of MagnaCut from multiple Crucible “heats” and sent them to Erasteel so that they could have appropriate offsets to match the Crucible material. We will continue to monitor the performance of the new MagnaCut material because of the distributions. If heats on the low end or high end of certain elements are not performing well in one performance category or another we could shift the target or tighten the acceptable ranges. This is the side of development and quality control that is often not seen by the end customer and is probably not very exciting.

Erasteel vs Crucible MagnaCut

One very important part of MagnaCut is its high corrosion resistance. So I tested with my standard 1% saltwater spray test. Most stainless knife steels will see some rust spots with this test. In this case neither the Crucible or Erasteel material showed any rust spots:

I also tested the hardening response. For a given heat treatment the hardness was very similar, perhaps the Erasteel material was slightly higher:

Surprisingly (based on the Z-Wear and M390 results), the toughness of Erasteel MagnaCut was significantly higher:

You can see that the Erasteel MagnaCut was significantly higher, matching AEB-L at ~62 Rc, and exceeding it at ~64 Rc. I wouldn’t necessarily extrapolate that up to AEB-L levels at 60-61 Rc but in that hardness range it was very good. Comparing with non-stainless steels this also makes Erasteel MagnaCut look more competitive:

While Crucible MagnaCut was a bit below the best results of CPM-CruWear and Z-Wear, the Erasteel version matches or exceeds it. In my knife steel ratings I had given MagnaCut a “7” for toughness and CPM-CruWear an “8,” so this is exciting. MagnaCut has a similar carbide volume to CPM-CruWear but has even smaller carbides so it was always a bit disappointing that the measured toughness wasn’t matching it. Perhaps this was a case where oxide inclusions were reducing toughness slightly in the Crucible version. Erasteel MagnaCut even roughly matched the new Bohler K888 steel, advertised for its high toughness, and tested better than steels like Vanadis 4 Extra. One thing to note is that toughness differences are basically on a “log scale,” meaning that differences at small values are bigger than those at large values. So the difference between 5 and 10 ft-lbs is about the same as between 10 and 20 ft-lbs.

One difference I noted in toughness testing is that using an austenitizing temperature of 2150°F (1175°C) and then tempering to desired hardness led to better toughness than lower austenitizing temperatures. With Crucible MagnaCut the optimum property balance was with 2050°F (1120°C).

You can see that for a constant toughness of ~20 ft-lbs that the hardness can be higher for that same toughness with a higher austenitizing temperature, about a 2.5 Rc increase.

Summary and Conclusions

The MagnaCut now being produced by Erasteel matches or exceeds the properties of the previous Crucible version. Specifically the toughness showed an improvement. We will continue to monitor the properties of the new material to ensure the performance meets expectations with the new manufacturing partner.

The post Testing Erasteel MagnaCut (vs Crucible Original) appeared first on Knife Steel Nerds.

  •  

Testing Tamahagane – Traditional Japanese Steel

Patreon

Thank you Patreon supporters! Through Patreon support I was able to pay for metallography and for the consumables for making coupons and running the CATRA experiment. If you want to support more knife steel research please join us at Patreon.com/KnifeSteelNerds

Video

Here is the video version of the following information:

What is Tamahagane?

Tamahagane is the name used in Japan for steel made with their centuries-old process. There are several videos available online to see the process such as this one. It starts with “iron sand” which is a naturally occurring form of iron mostly composed of magnetite, Fe3O4, though can also contain some hematite (Fe2O3) and other constituents like quartz and titanium dioxide [1]. One nice thing about magnetite (as the name suggests) is that it is magnetic, so it can be relatively easily separated from other minerals with magnets. The iron sand is then “smelted,” which is the process of reducing the oxide ore to the base metal, in this case, iron. The smelting is performed in a traditional furnace called a tatara. A clay tub is used which is layered with charcoal and the iron sand [2]. The charcoal acts as a reducing agent to turn the magnetite into iron, and also is a carbon source to turn the iron into steel (steel is iron plus carbon). The charcoal reduces the steel because carbon monoxide and carbon dioxide forms when it burns in air. The carbon monoxide (CO) reduces the magnetite to iron [3]. At the end the clay vessel is broken and the tamahagane is removed, which is in the form of rough and porous sponge-like pieces that also contains slag (large undesirable inclusions). The swordsmith separates pieces by “grade” which corresponds to the approximate content [4]. The grade is determined by color and also the fracture appearance [4]. The swordsmith then forges the pieces gently, and then folds and forge-welds them multiple times to eliminate porosity, remove some slag, even out the carbon content, and break up inclusions and impurities.

The “sponge-like” pieces of tamahagane after smelting. Picture from Wikipedia.

Soo all of that describes the manufacturing process. Ultimately tamahagane is a simple carbon steel. It is even simpler than a typical carbon steel like 1095 or White #1, because it is lacking intentional additions to those steels of manganese and silicon. So the steel has carbon of some content (described next) and then only trace amounts of other elements.

While there are a few individual swordsmiths that make their own tamahagane, most of the tamahagane produced in Japan comes from Nittoho tatara in Shiname Prefecture, the last of its kind. All tamahagane production had ceased by World War II. But this facility was restarted in 1977 and continues to produce the traditional steel for Japanese swordsmiths.

Published Tests of Tamahagane

Carbon Content and Composition

The cutting edge of Japanese swords has typically been found to be around 0.5-0.8% carbon [2, 5-9]. However, there are different types of construction used in Japanese swords, such as the “kobuse” method that uses a low carbon core and a higher carbon sides and cutting edge. Thus, the low-carbon pieces of tamahagane can be used in these low-carbon portions, giving the blades greater ductility and reducing the chance of catastrophic breakage. Measurements of the core carbon content have returned values between 0.01% [7-8] and 0.2% [2]. Sometimes steel with a carbon content in between these two extremes is used on the sides [2,7-8].

Schematic of “kobuse” construction from [3]

However, the carbon content is not always perfectly distributed throughout. Analysis of a modern kogatana knife (utility knife) produced by Sadanao Mikami had a range of carbon from 0.6% on one end to 2.0% on the other [5-6]. The uneven carbon content can come from distributions within the original pieces, mixing of low carbon and high carbon pieces (often done intentionally), and performing an insufficient number of forge-folding operations to even out the carbon. They reported that the average carbon content was 1.03% for the entire knife [5]. There were also small amounts of other elements:

Composition of modern kogatana by Sadanao Mikami [5]

Microstructure and Hardness

Japanese swords are produced to have a “hamon,” a visible line that distinguishes between a soft spine and the hard cutting edge. Thick clay is applied to the blades at the spine to slow the quench rate so that it does not harden. The hard phase at the edge is martensite, and the soft phase is pearlite. At the hamon transition, there is a combination of martensite and pearlite. The low carbon core contains large amounts of soft ferrite. The pearlite content of the core is determined by the carbon content, more carbon means more pearlite.

Images of microstructure from a “modern” sword (1945) and an “old” sword (~600 years old) at different locations [9]

Micrographs of a ~600 year old sword [7]

Studies on the hardness of Japanese swords correspond to these differences in microstructure and carbon content. Typically, the hardness at the edge is between 600-900 HV [2,3, 5,7, 9] and the spine is between 100-300 HV [2, 3, 7, 9]. This corresponds to about 55-67 Rc at the edge and 0-30 Rc at the spine (Note: Rockwell C hardness only reliably goes down to 20).

Microhardness values of ~600 year old sword [7]

Microhardness of a “Koto” style Japanese blade (before 1596 AD) [3]

Microhardness from the 1945 and 600 year old swords [9].

Impurities, Inclusions, Forge Welding, and Folding

A study was performed along with swordsmith Sadanao Mikami on the effect of forging and folding on impurities and inclusions in tamahagane [10]. The process is shown in the figure below:

The forge welding and folding process used in Ref. [10]

The swordsmith started by hammering chunks of tamahagane into sheets, then cutting those sheets into chips. The chips are sorted by carbon content by hitting them with a hammer. High carbon chips break and low carbon chips don’t. The low carbon chips were stacked together and forged together into a bar, then cut and restacked six times (A1-A6); this was repeated with the high carbon chips (B1-B6). Then the low and high carbon bars were stacked together and forge welded together, followed by cutting, restacking, and forge welding six more times (C1-C6). The microstructure became more evenly distributed through the forge welding process as the carbon content became more equalized, as shown in the following images:

Microstructure evolution of tamahagane after forge-folding operations [10]

One common claim of folding and forge welding is the elimination of inclusions, oxides and slag that are present in the original tamahagane pieces. The researchers found that while bands of FeO were present in A1 and B1 from oxides present in the original pieces, they were not found in A6 or B6. In other words, the FeO bands were eliminated by further forging and forge welding. They were originally present in bands from forge welding flat pieces together. They also found silica (SiO2) and Fayalite (Fe2SiO4) inclusions in the steel. The silica particles were less than 1 micron and the Fayalite inclusions were 16-20 microns in length in the A1 and B1 samples. The thickness of the Fayalite bands was significantly smaller than the FeO, about two microns.

Iron oxide bands forge welded into tamahagane during initial forge welding

The Fayalite was reduced from 16-20 microns long in the A1/B1 specimens to 14-15 microns in the A6/B6 specimens. These were further reduced to 13.1 microns in the C1 specimens and down to only 8.2 microns in the C6 specimens. So while forge welding and folding did not significantly reduce the volume fraction of Fayalite inclusions, they were reduced in size, more isotropic (round), and more evenly distributed after that process.

Inclusions in tamahagane steel in the C1 condition (one forge weld of low and high carbon steel), left, and after six folding and forge welding operations, right [10]

In a study on a kogatana knife produced by Sadanao Mikami had relatively homogenous oxide inclusions in the size range of 5-10 microns [5]. They reported a volume of 4-7% inclusions.

Oxide inclusions in modern tamahagane knife [5]

Analysis of a ~600 year old sword [7] found an inclusion content of 0.8-1.9%, which they found to be much higher than the content in a modern production steel (labeled “ordinary steel”).

Volume percent of inclusions in ancient sword vs modern steel [7]

Micrographs of inclusions in ancient sword [7]

Analysis of another ancient sword found an inclusion volume of 1.1% [3]. The authors claimed that this inclusion content is low enough to avoid a “significant reduction in its toughness.”

Inclusions in pre-1596 AD sword (cross-hair scratch added intentionally) [3]

Strength and Toughness

Tensile tests of a sword by swordsmith T. Takaichi were performed and compared with a conventional carbon steel with similar carbon content of 0.55% C [2]. They found that in testing of the steel before heat treating that the conventional steel (S55C) had greater utility than the tamahagane sword steel (S1). When observing the fracture surfaces, they found oxides in the tamahagane and they speculated that it was these oxides that led to the lower ductility.

Stress-strain curves and fracture appearance of tamahagane sword steel (S1) and conventional steel (S55C) [2]

In tests of a ~600 year old sword and a 1945 sword, they measured the strength and ductility of the swords with a 4-point bending test [8-9].

4-point bend test of tamahagane swords [9]

They found the ancient sword to form a crack at around 0.88 ton-force, but the blade did not fully break and continued bending until final fracture. The 1945 sword broke at 2.62 ton-force and did not have the load drop from cracking that the ancient sword had. They calculated the bending strength of the swords as 2552 MPa for the ancient sword and 4645 MPa for the 1945 sword. They claimed that these results are “in a range of performance tool steel” [8]. The hardness of the cutting edges were similar in the two swords. Instead, they said the difference in measured strength was because the 1945 sword had a 5 mm hardened area while the ancient sword had only 1 mm of hardened area (see earlier microhardness charts).

I didn’t find much other toughness testing of tamahagane so comparisons between this traditional steel and modern carbon steels are in short supply. I found one study of miniature charpy specimens taken from a Japanese sword [11], but they did not compare with similar tool steels. Furthermore, the values at the edge of the knife where we would probably be more interested were essentially zero:

Image taken from [11]

Effect of Carbon Content on Final Properties

While there seems to be a consensus that the cutting edges of tamahagane Japanese swords are in the range of 0.5-0.8% carbon or so, I am not sure if the carbon content was and is that consistent. There was the one study on the tamahagane knife where they found carbon values as high as 2% within the same knife that read 0.6% in other locations [6]. I also found a study on different iron sand use at the Nittoho tatara (the last major facility remaining), and found that they had moved to a different source of sand that resulted in higher carbon and lower impurities [4]. So I think there is reason to believe that carbon content of tamahagane has gone up in recent decades.

The carbon content is very important to steel properties. One of the best known is the effect of carbon on the resulting as-quenched hardness. The higher the carbon content, the higher the hardness, though it levels out around 0.6% carbon:

Image from [12]

Carbon has an equally strong effect on impact toughness, even when tested at the same hardness for different low alloy tool steels:

Higher carbon also gives steel more iron carbide (cementite) which gives it greater wear resistance. This can give knives greater edge retention because edge wear is slowed. However, for a sword this wear resistance is not really beneficial, and toughness is a much more important property. So the 0.5-0.7% range of carbon would be about optimal for a sword, given the high combination of hardness/strength and toughness that you get from this microstructure. But for smaller knives, kitchen knives, etc made with tamahagane higher carbon could be beneficial for wear resistance.

1.25%C steel with significant carbide content (white particles)

0.6%C steel with almost no visible carbide

My Tamahagane for Testing

I recently went to Japan and took a class from Yuya Nakanishi, also called Masahiro. You can watch a video of our trip to Japan and making the “kogatana” (a utility knife). We took home our two knives that we made with him. However, I also wanted to test the steel for toughness which would be difficult with just the knife, as the standard toughness test uses rectangles. So I asked him if I could have a piece for toughness testing and he let me have one. This piece had already been through the forge welding and folding process. I also asked him what temperatures to use for heat treating and he told me 780°C for austenitizing and 180°C for tempering. I normalized and annealed the piece first, and followed his recommendations by austenitizing for 10 minutes, quenching in water, and tempering twice for one hour at each time.

Image from https://morinokyoto.jp/masahiro_en/

Carbon Content

I measured the broken toughness specimen with LECO combustion for carbon and sulfur content and got 1.06% carbon and 0.001% sulfur. This carbon content puts it into a range similar to White #2 (1.05-1.15%C). This is a good range for a utility knife, though as explained above would be on the high side for a sword. I am not sure if this is because Masahiro intentionally used higher carbon tamahagane for these smaller knives, or if it is due to carbon fluctuations, or higher carbon tamahagane being made at the Nittoho tatara. If I hear back from Masahiro I will update the article. This is very close to the carbon content in the kogatana by Mikami of 1.03% [5], which perhaps provides evidence that the carbon content of tamahagane has increased from older blades. I wasn’t able to measure other elements because of the size of the steel that I had.

Micrographs

The carbide structure looks consistent with the measured carbon content of 1.05%. It has a significant amount of small and evenly distributed carbides, but a smaller volume than the higher carbon 26C3. It looks closer to O1 and 52100, though the carbides are even finer in the tamahagane.

Micrograph of the heat treated tamahagane

O1 steel

52100 steel

Looking at a lower magnification micrograph, the carbide structure appears relatively consistent throughout. There are no visible layers from the forge-folding process. There is a “bright spot” in the upper left portion of the image. Higher magnification reveals that this is not carbide clusters but either an etching artifact or retained austenite.

Lower magnification of tamahagane

Impurities and Inclusions

The inclusion content of the tamahagane provided to me is very low, lower than reported inclusion contents in the journal articles that I cited. Using threshold measurements I estimate the inclusion content to be around 0.1%. I am not sure why this steel is so much “cleaner” than those analyzed in the other studies.

Polished (unetched) surface of tamahagane. Black particles are inclusions.

There is a small amount of orange, square/rectangular particles in the steel. These are likely titanium nitride (TiN) as these particles are typically yellow/orange and angular [13]. Iron sand typically has TiO2 in it [1], and the Mikami blade had 0.03% Ti in it [5], so the presence of TiN is not entirely unexpected. Titanium and nitrogen have a strong affinity for each other, and these particles are often found in steels with small titanium additions.

Titanium nitride particles (TiN)

Hardness

The hardness of my toughness coupon was 64.6 Rc. This is relatively high in hardness, maybe even a bit high for a utility knife. However, it is within a reasonable range, and would provide very good cutting and edge retention. This lines up closely with tempering of other simple high carbon steels, such as 1.25% carbon steel 26C3, shown below. The 26C3 is somewhat lower in hardness, though this steel was tempered in another oven. My furnace is very good at maintaining a consistent temperature during tempering, so “overshooting” is less common.

I am not able to measure the hardness of the edge of the knife that I made at Masahiro Tantojo, as it is only hardened at the edge. It would require cutting it apart and using microhardness measurements to see. Since the knife was tempered by eye by the swordsmith it could be significantly different in hardness. The tempering was performed for a very short period, until it reached a temperature where water would sizzle when he touched the blade. My guess is that it is higher in hardness, somewhere between 65-67 Rc. However, if the carbon content is significantly lower in the blade it is possible that it would also be lower in hardness.

Toughness

Given the relatively high hardness of 64.6 Rc, the toughness was not chart topping. I measured 5.8 ft-lbs. However, this is a relatively high value for that level of hardness, as you can see when compared against other low alloy steels here:

As you can see the toughness falls right on the same line as 26C3 (green line in the upper image). So the tamahagane appears to be behaving similarly to conventionally produced low alloy high carbon steels. Overall I think this is a good result considering that some studies I cited before showed a potential reduction in toughness from oxides.

Edge Retention

Comparing the edge retention is a bit tricky since the kogatana design is different than the standard test knife that I use for CATRA testing. This knife is thinner behind the edge, about 0.010″ (0.25 mm) after sharpening, while our test knives are around 0.015″. This gives the thinner knife an advantage for a given edge angle, as shown in this earlier study on 154CM steel:

There is also the complication that I do not know the hardness of the kogatana knife, my guess is it is in the range of 65-67 Rc. When I tested it with CATRA I got 370 mm, which would also lend credence to the hypothesis that it is on the upper end of hardness.

There aren’t many low-alloy steels I have tested that would be in that hardness range. The light grey dotted lines show the approximate relationship between hardness and edge retention. So you will notice that the tamahagane is on the same line as most of the other low alloy steels, especially after accounting for the knife being thinner behind the edge. This is not too surprising given that most of the low alloy and carbon steels have tested in a similar range after accounting for hardness.

Tim Zowada Information

Tim is a bladesmith who makes his own bloomery steel using iron sand from Lake Superior. He was an author on one of the cited papers above along with Dr. John Verhoeven. He had the following comments after reading my report:

Here are a couple things that might be helpful. In general:

1. The final carbon content is determined by the average initial carbon content and the number of folds. More folds decrease the carbon content. The outside of the billet will decarburize during forging. That decarb layer is folded in with each weld, decreasing the average carbon content. Plus, the oxidation of the billet (scale) will decrease the overall size of the billet during all the folding and welding. For high quality steel, the typical number of of folds will be between 10 and 15. It ends up being a balancing act based on experience. Yoshindo Yoshihara prefers about 0.7% carbon for his swords. His brother prefers 0.6%. Maybe I have that backwards. The Art of the Japanese Sword (Yoshihara) is an excellent book that you should own. I’m not sure why the carbon content varied so much in your blade. My best guess is a low number of folds. A quick nital or ferric chloride etch would tell. You would be able to see lighter and darker bands of varying carbon content. Typically, the carbon content is pretty much homogeneous through the bar by about eight folds.

2. High hardness and low abrasion resistance is an advantage for my straight razor work. At 65 HRC, the blades hold up very well against whiskers. But, with the low abrasion resistance, a clean leather strop will remove enough metal to keep them sharp. They don’t need to go to the stones very often.

3. Like many things, the final carbon content and quality of the steel will vary from smith to smith, and batch to batch. I think what you got was a good representation of high carbon (1.0%) tamahagane.

Summary and Conclusions

Reviewing the prior studies on tamahagane, researchers of this material have been pretty realistic about its properties. At its best, tamahagane performs like other simple carbon steels. The potential for higher oxide inclusion content potentially limits its toughness, though in my own experiments it was roughly in line with the toughness you would expect for a steel made with modern methods. It is very interesting to learn about traditional methods for making steel and how they compare to the more advanced methods that we have developed since.


[1] Tanii, Hiroshi, Tadahiro Inazumi, and Keiichi Terashima. “Mineralogical study of iron sand with different metallurgical characteristic to smelting with use of Japanese classic iron-making furnace “Tatara”.” ISIJ international 54, no. 5 (2014): 1044-1050.

[2] Okayasu, Mitsuhiro, H. Sakai, and T. Tanaka. “Mechanical Properties of Samurai Swords (Carbon Steel) Made Using a Traditional Steelmaking Technology (tatara).” Journal of Material Sciences & Engineering 4, no. 2 (2015): 1-6.

[3] Verhoeven, J. D., and Tim Zowada. “Comparison of Two Swords of Antiquity: The Japanese Sword and the Muslim Crucible Damascus Sword.” Metallography, Microstructure, and Analysis 12, no. 6 (2023): 934-943.

[4] SUZUKI, Takuo, and Kazuhiro NAGATA. “Effect of the charge of” Komori” iron sand on the properties of” Tamahagane” steel produced by” Tatara” operation.” Tetsu-to-hagané 85, no. 12 (1999): 911-916.

[5] Das, Ananda Kumar, Takuya Ohba, Shigekazu Morito, and Muneo Yaso. “Evidence of Lath Martensite in High-C Japanese Sword Produced from Tamahagane Steel by Tatara Process.” In Materials Science Forum, vol. 654, pp. 138-141. Trans Tech Publications Ltd, 2010.

[6] Matsumoto, Chihiro, Ananda Kumar Das, Takuya Ohba, Shigekazu Morito, Taisuke Hayashi, and Go Takami. “Characteristics of Japanese sword produced from tatara steel.” Journal of Alloys and Compounds 577 (2013): S673-S677.

[7] Yaso, Muneo, Toshifumi Takaiwa, Yoshihiro Minagi, Kunichika Kubota, Shigekazu Morito, Takuya Ohba, and A. K. Das. “Study of microstructures on cross section of JAPANESE SWORD.” In European Symposium on Martensitic Transformations, p. 07018. EDP Sciences, 2009.

[8] Yaso, Muneo, Yoshihiro Minagi, Toshifumi Takaiwa, Kunichika Kubota, Tsuyoshi Kanaizumi, Takuya Ohba, Shigekazu Morito, and Taisuke Hayashi. “Study of Metallurgy and Mechanical Property on Japanese Sword.” In Materials Science Forum, vol. 738, pp. 222-227. Trans Tech Publications Ltd, 2013.

[9] Yaso, Muneo, Toshifumi Takaiwa, Yoshihiro Minagi, Tsuyoshi Kanaizumi, Kunichika Kubota, Taisuke Hayashi, Shigekazu Morito, and Takuya Ohba. “Study of Japanese sword from a viewpoint of steel strength.” Journal of Alloys and Compounds 577 (2013): S690-S694.

[10] Takami, Go, Takuya Ohba, Shigekazu Morito, and Ananda Kumar Das. “Microstructural observation on materials of the japanese sword under fold-forging process.” In Materials Science Forum, vol. 654, pp. 134-137. Trans Tech Publications Ltd, 2010.

[11] Misawa, Toshihei, and Shin-Ichi Komazaki. “Ductile-brittel transition evaluation of Japanese sword and weld metals using miniaturized impact specimens.” In European Structural Integrity Society, vol. 30, pp. 119-125. Elsevier, 2002.

[12] Krauss, George. “Martensitic transformation, structure and properties in hardenable steels.” Metallurgical Society AIME,(1978): 229-248.

[13] Descotes, Vincent, Thibault Quatravaux, Jean-Pierre Bellot, Sylvain Witzke, and Alain Jardy. “Titanium nitride (TiN) germination and growth during vacuum arc remelting of a maraging steel.” Metals 10, no. 4 (2020): 541.

The post Testing Tamahagane – Traditional Japanese Steel appeared first on Knife Steel Nerds.

  •  

Pop’s ProCut – A New Carbon Steel for Knives

My steel research is supported through Patreon. Patreon supporters saw the news on Pop’s ProCut before anyone else. There is currently an article about the upcoming MagnaMax only available on Patreon.

Video

Here is a video version of the following information:

Development

In March 2024 Joey Berry of Pop’s Knife Supply called me and said he wanted to develop a new steel. He said that their most popular steel was 80CrV2 and so he wanted to make “80CrV3.” “You mean 80CrV2 but with a little more vanadium?” He said no but some kind of “sequel” to 80CrV2 that would be more exciting. I told him that doesn’t give me much to go off of but I would think about whether I had any good ideas along those lines. I thought about gaps in the market in the area of low alloy knife steels (“Carbon steel”) that would also be usable by the knifemaker that is buying 80CrV2. It occurred to me that our selection of high nickel steels is very limited; 15N20, L6, and 8670 are pretty much it. These steels are high in toughness and offer good hardness to go with it, but have no real wear resistance to speak of. 80CrV2 is in a similar position just without the nickel. I thought if we added some tungsten and vanadium to a high nickel steel we could make the steel more balanced; give it some wear resistance along with the high toughness. Those carbide pinning elements would mean that the steels are more beginner friendly for forge heat treating. 15N20, for example, already sees grain growth around 1500°F (815°C) and so its toughness drops very rapidly even when only slightly overheated. If the tungsten and vanadium were kept in check the forgeability, grindability, and polishability would remain high. This would also offer an alternative to other tungsten/vanadium steels like Blue #1, V-Toku2, Wolfram Special, 1.2519, and others. Those steels don’t have much toughness to speak of, so we could combine the best of the nickel steels with the best of the tungsten/vanadium steels. Another exciting element with the high nickel is the possibility to use the steel in pattern-welded Damascus as a “bright” layer. This gives an option for a higher wear resistance steel with better edge retention for that component of the Damascus. I told Joey about my idea and we decided to move forward with it.

We took the composition I came up with to a steel mill in Europe and they agreed to make it. I spent a bunch of time working on optimal annealing for the somewhat similar 15N20 based on the limitations of their production annealing process. Based on that we generated an annealing procedure to make the steel respond well to forge heat treating.

Composition and Tungsten/Vanadium Carbides

Here is the composition of Pop’s ProCut compared with other grades in its category. The far right column says “MC (%)” which is a calculation of how much total vanadium and tungsten carbide each steel contains after heat treating. One thing you will notice is that since tungsten is a heavy element it does not contribute as much to the MC as you might expect. For example, CruForgeV with 0.75% vanadium has more MC than Wolfram Special which has ~2.25% tungsten. ProCut uses a combination of vanadium and tungsten in a similar fashion to O7 and 1.2519 steels. So it has similar MC to steels like Blue #1, 1.2519/O7, and Wolfram Special, and more MC than Blue #2 and O1. The other nickel nickel steels (15N20, L6, and 8670) of course do not have any MC. These very hard carbides give the steel wear resistance.

Austenitizing, Tempering, and Hardness

A major goal for this grade was to be “easy” to heat treat with a forge. This requires a wide range of austenitizing temperature where full hardness is achieved while avoiding a toughness drop with higher temperatures. 80CrV2 steel varies a lot with starting microstructure, and two of the mills that make the steel lead to very different heat treating response:

So we wanted to avoid this issue that 80CrV2 sees. We did this by keeping the chromium low and also working with the manufacturer to dial in the annealing procedure so that carbides aren’t too coarse (making them difficult to dissolve). I also compared the austenitizing response with my recommended anneal (described later):

You can see that the hardness reaches its maximum around 1475°F and then does not change above that temperature. If using the anneal I recommend the microstructure is a bit finer and so this can be dropped even further to 1375°F. Thus for heat treating in a forge you can heat the steel to “a shade brighter” after reaching nonmagnetic and the steel will fully harden. If you forge and follow the recommending normalizing and annealing procedure you can even quench from nonmagnetic if you wish.

If the steel is austenitized in that range (1475°F or higher) the tempering is roughly the same regardless of the austenitizing temperature. Here are datapoints for both 1550°F and 1625°F:

You can see that the hardness is relatively high, still 64 Rc after tempering at 300°F, which is generally as low as I recommend for tempering most any steel. With a 450°F temper the steel is still above 60 Rc.

Toughness

Austenitizing

In our heat treating and toughness experiments we found three different regions of toughness behavior:

Below 1500°F, the steel shows an increase in toughness with increasing temperature. From 1500-1575°F the toughness is roughly flat. 1625°F and above shows a big jump in toughness where it is flat again up to at least 1675°F. The reason for this behavior we figured out by looking at the microstructure. These images were taken by knifemaker Shawn Houston of Triple B Knives:

1425°F, 400°F temper

1475°F, 400°F temper

1600°F, 400°F temper

You can see that the carbide content is significantly reduced by austenitizing at 1475°F as opposed to 1425°F. This significant change in cementite (iron carbide) raised toughness. Then when the temperature is further increased to 1600°F and above, virtually all of the cementite is gone and all that remains is the small volume of hard vanadium and tungsten carbides. The presence of these small carbides is what prevents grain growth even at high temperatures. The carbides “pin” the grain boundaries.

15N20 and L6, in contrast, show a drop in toughness at much lower temperatures because they do not have those carbides to pin grains. The steel 1.2519 does have the W/V carbides but it sees a drop in toughness above 1500°F because it gets excess carbon in solution, leading to plate martensite. The carbon content in ProCut is controlled so that the matrix carbon does not reach excessive levels even at high temperature. This gives ProCut a very wide austenitizing range.

Tempering and Toughness

Like many other knife steels, ProCut sees a peak in toughness with a tempering temperature of around 450°F (230°C). Above that the toughness drops due to a phenomena called “tempered martensite embrittlement” which happens in all steels. There is lower toughness with tempering at lower temperatures as well, of course, corresponding with the higher hardness. The behavior of toughness with tempering temperature is roughly similar whether using the higher or lower austenitizing temperature range.

Hardness vs Toughness

This creates two different heat treating ranges, where the steel can be austenitized high (1625-1675°F) to max out toughness with some cost to wear resistance and edge retention, or austenitizing lower (1475-1575°F) to retain more carbide for wear resistance. The steel still maintains a toughness advantage vs previous tungsten/vanadium steels due to the nickel addition and controlled carbon content with the lower austenitizing range. However, with the high austenitizing range it achieves levels of toughness similar to 8670, 15N20, and L6 but with enhanced wear resistance due to the small tungsten and vanadium carbides.

To compare with other steels you can look at the following chart:

Grinding and Polishing

I don’t have a quantitative test for grindability. Reports from knifemakers so far say that grinding and polishing is very easy with the steel. Some low alloy steels developed for higher wear resistance like CruForgeV are more difficult to polish due to relatively large vanadium carbides that are found relatively frequently. This steel we controlled the W/V content to try to avoid large carbides. Because of the limitations of standard steelmaking (as opposed to powder metallurgy) there are still very occasional larger carbides but they are much rarer than a steel like CruForgeV. So far those few carbides don’t appear to be affecting polishing and finishing.

A lower magnification image of ProCut showing that large carbides aren’t observed most of the time

One of the rare large carbides in ProCut

A micrograph of CruForgeV showing large carbides. Notice there is a magnfication difference vs the ProCut images.

Quenching, Oil Selection, and Hamon

The “hardenability” of ProCut is relatively high, which I also found in testing of 15N20. The high nickel content gives it this hardenability. Air cooling from 1600°F with 1/8″ steel resulted in 60.7 Rc, though from lower temperatures like 1350°F the hardenability is lower (I measured 35.3 Rc). This means that ProCut can be quenched in virtually any quenching oil, even canola, and with relatively thick cross-sections.

This high hardenability means that ProCut is not well suited for developing a hamon. The best choices for a hamon are low hardenability steels like 1095, W2, and 26C3. I won’t say it is impossible to develop a hamon but there are better choices. It is likely still fine for other differential methods like an edge quench.

Forging, Thermal Cycling

Maximum forging temperatures are most greatly affected by the carbon content. High carbon steels are easier to overheat, leading to crumbling while forging. The carbon content of ProCut is limited to ~0.87% so this is not a huge factor with ProCut. For safety I put in the datasheet to limit forging to 2200°F (1200°C). Some knifemakers, especially Damascus makers, push the boundaries of forging temperatures and this can be dangerous. Like with other steels, if you continue to forge when the steel gets too cold this is also a danger in terms of cracking. I haven’t heard a lot of feedback in this area so let me know how the steel behaves for you. The high hardenability means that the steel can sometimes harden in air while cooling from the forging temperature. This can lead to cracking if there are stress risers in the blade.

The “thermal cycling” procedure for ProCut is relatively simple. Like with other steels I prefer to do a single normalize and anneal, so only two steps. I have written about this procedure in past articles. The normalizing step is for dissolving any undesirable carbides and other structures. For this steel it would be in the range of 1600-1650°F where the cementite is dissolved. With a furnace you can hold at this temperature for 10-15 minutes before air cooling. With a forge by eye you just need to heat somewhere into that range or a bit higher.

The annealing procedure is then done by heating to nonmagnetic and slow cooling. I recommend faster cooling rates than is typical for datasheets and this type of anneal is called a “Fast DET” anneal. For simple heat treatments you can slow cool either in a furnace or in an insulating media like vermiculite (available in the garden section of home improvement stores). I tried a range of cooling rates in my furnace. I held the steel for 30 minutes at 1350°F and slow cooled at different rates to measure the annealed hardness. At 50°F/hr cooling the resulting hardness was 23.9 Rc. After 500°F/hr the hardness was 24.5 Rc. I also tried setting the furnace to 1000°F/hr but it only maintained that cooling rate until about 1250°F and slowed from there, the average rate of cooling was about 680°F/hr. That resulted in 26.2 Rc, which is plenty soft enough. Shawn Houston did an anneal with 250°F/hr and he measured 21.2 Rc. Here is the microstructure after normalizing and annealing at 1350°F for 30 minutes, and cooling at 250°F/hr:

Normalized and “Fast DET” annealed microstructure of ProCut (21.2 Rc)

“As-received” annealed microstructure of ProCut (12 Rc)

You can see that the faster annealing procedure results in a finer microstructure which is why the austenitizing response was different (see the prior as-quenched hardness chart). The toughness was still relatively similar despite the very different starting microstructure (see the toughness vs austenitizing temperature chart). Those datapoints were generated using a 100°F/hr anneal which is what I recommended in the datasheet. Somewhat faster and slower cooling rates would have a similar result.

Use in Damascus

The high nickel content means that ProCut is a good replacement for 15N20 or L6 as a bright layer in pattern-welded Damascus. This gives an option for providing higher edge retention whereas 15N20 and L6 have almost no wear resistance apart from their hardness. An initial forging experiment with 1084 and ProCut resulted in excellent contrast:

Edge Retention

Pop’s ProCut did surprisingly well in the CATRA test. The heat treatments performed were 1650°F with a 450°F temper (61.2 Rc), and 1500°F with a 300°F temper (64 Rc). As I have written about before, CATRA is not the best for low alloy steels because the sand particles in the test media are harder than cementite (iron carbides). Even with different media they wouldn’t be at the top of the chart but they would be a bit better. It could be that the relatively low amount of cementite in ProCut helped for the CATRA test. But even if that were the case if we compare with another steel with low cementite content like 8670 or 1095, there was a significant boost to edge retention through the tungsten and vanadium additions. Perhaps with the lower carbon compared with other W/V steels meant that there was less of tungsten and vanadium found in the cementite, allowing them to form more of the hard WC and VC carbides.

Toughness-Edge Retention Balance

With the high toughness plus the unexpectedly good CATRA numbers the ProCut looks very good compared with other low alloy steel options:

Corrosion Resistance

This is a non-stainless steel and should not be expected to be stainless. People say that the 2% nickel in 15N20 gives it somewhat better corrosion resistance than carbon steels but I have not developed a test for comparing corrosion resistance of low alloy steels.

Cryo

There is a certain lore out there with knifemakers claiming that some steels “need” cryo and other steels “don’t benefit” from cryo. Part of this lore is that low alloy and carbon steels are in the “don’t benefit” category. Simple carbon steels and low alloy steels still see an increase in hardness with cryo, typically 0.5-2 Rc depending on the steel and the heat treatment. There is a small cost to toughness because of the increase in hardness. ProCut is the same. As an example of another low alloy steel we experimented with see 52100. I did experiments from 1500°F and 1650°F and found, as expected, that hardness increased. The higher temperature led to a bigger bump from cyro which is also typical. None of the edge retention or toughness tests I showed in the article so far used cryo in any of the heat treatments. But if you want even higher hardness for edge retention and strength you can add a cryo step after quenching.

Comparisons to Other Steels

1084 and 15N20

These steels are relatively “easy” to heat treat in that you can heat them up and quench them and get full hardness. However, they are very easy to overheat leading to grain growth and a drop in toughness. They also have almost no carbide thus having very little wear resistance.

80CrV2

This steel is also lacking in wear resistance though overheating is not much of an issue because of the vanadium addition. It also varies a lot between manufacturers and needs more temperature prior to quenching making it more difficult to perform a forge heat treatment.

52100

In the lower austenitizing range (for higher wear resistance), ProCut compares favorably with 52100 in terms of properties. 52100 has a very good combination of toughness and wear resistance. ProCut is easier to heat treat for an amateur knifemaker and also has the option of the high toughness heat treatment.

O1 and 1095

These are old standard steels. O1 has the benefit of being “oil hardening” so it is easier to quench. I have found both to be very sensitive to overheating because of excess carbon in solution. See my article on O1.

5160, 8670, and L6

These steels have significant chromium additions so they are more difficult to heat treat in a forge. They also don’t have any carbide left over after heat treating and thus their wear resistance is very low.

Blue #2, Wolfram Special, 1.2519

These steels have similar wear resistance for edge retention but significantly lower toughness and do not have the benefits of being beginner friendly.

ApexUltra

This is another low alloy steel I helped develop. It has significantly higher wear resistance and attainable hardness than ProCut, which also means lower toughness. I would recommend ApexUltra for those looking for maximum performance in the “carbon steel” category. Though I wouldn’t call it a difficult steel, it is best for makers that have a bit of experience first.

Heat Treatment Recommendations

In a Forge

Heat to “one shade brighter” after reaching nonmagnetic, quench in oil (most types are fine), and temper twice for one hour each time at 300-450°F (150-230°C) to desired hardness.

In a Furnace

Maximum toughness: 1650°F (900°C) for 10-15 minutes.

Higher edge retention: 1500°F (815°C) for 10-15 minutes

Quench in oil (most types are fine), and temper twice for one hour each time at 300-450°F (150-230°C) to desired hardness.

Thermal Cycling after Forging

1625-1675°F for 10-15 minutes, air cool. Without a controlled furnace, heat into that rough range and establish an even temperature distribution prior to cooling.

1350°F for 30 minutes, cool at 100°F/hr to 1100°F. After that it can be cooled more rapidly. Without a controlled furnace, heat to nonmagnetic and slow cool such as in vermiculite.

Summary and Conclusions

I am happy with how Pop’s ProCut turned out. It offers good balanced performance when compared with other low alloy non-stainless steels. Better edge retention than 1095, O1, 80CrV2, L6, 15N20, etc. And depending on the heat treatment its toughness approaches 8670, 15N20, and 5160. And on top of this it is beginner friendly, being easy to heat treat, grind, and finish.

The post Pop’s ProCut – A New Carbon Steel for Knives appeared first on Knife Steel Nerds.

  •  

CPM-3V – Still the Best High Toughness Steel

Still working on getting an update to everyone about the status of knife steel after Crucible’s bankruptcy and the sale of many of the assets to Erasteel. Still more i’s to dot and t’s to cross.

If you would like to support future knife steel research then please come join us at Patreon.com/KnifeSteelNerds. You can get access to articles and videos early!

Video

Here is the video version of the following information:

History of CPM-3V

The thing most don’t know about CPM-3V is that it is a powder metallurgy version of an older conventional steel called Vasco Die. Vasco Die was patented by Harry Johnstin of VASCO in 1964 [1]. This was the first popular “8% Cr die steel” which created a new category. The most popular cold work die steels were (and are) A2 and D2. D2 is used for higher wear resistance and A2 is used for higher toughness. The 8% Cr is right in the middle between D2 (12%) and A2 (5%). And with the 2.5% vanadium for wear resistance and the relatively low carbon of 0.8% it has an interesting combination of properties, better overall than either A2 or D2. The steel was advertised as twice as tough as D2 while have ten times the wear resistance of A2. This created a new category of cold work die steel which is still seen today in steels like DC53 and Sleipner. You can read more about the history of Vasco Die and all of the developments that led up to it in my book The Story of Knife Steel. Vasco Die was never really used in knives, though the higher carbon version, Vasco Wear, did get used by some knifemakers, and by Gerber in some production knives. And of course CPM CruWear, the PM version of Vasco Wear, has also developed some popularity in recent years.

In the mid-1990s, Kenneth Pinnow and William Stasko of Crucible were looking to make a high toughness powder metallurgy tool steel. Up until that point, powder metallurgy steels had focused on high hardness high speed steels and creating new steels with higher wear resistance than was possible with conventional steelmaking like CPM-10V. Crucible’s highest toughness PM steel was CPM-M4 and that was basically an accident. Uddeholm had released Vanadis 4 in the late 1980’s to be a more balanced steel and its toughness didn’t even match CPM-M4. Uddeholm would later redesign this steel and call it Vanadis 4 Extra. Pinnow and Stasko realized they needed a steel with lower carbide volume. Powder metallurgy leads to higher toughness because it keeps the carbide size small, but to achieve the highest levels of toughness they needed to have less overall carbide. They experimented with a few compositions and found that a PM version of Vasco Die had excellent toughness and wear resistance.

It is somewhat surprising to me that they managed to patent this steel in 1997 [2] since Vasco Die had already previously been patented (though the patent had expired). It seems their claim was that the powder metallurgy process significantly changed the steel, and in more ways than just making the carbides smaller. With conventional casting of steel there is significant segregation of elements, and this led to relatively large chromium carbides which couldn’t be dissolved in Vasco Die. With powder metallurgy, the heat treated microstructure is free from chromium carbide and has only vanadium carbide instead.

Images from 3V patent showing CPM-3V (Fig. 1) and Vasco Die (Fig. 2). The larger carbides labeled “C” are chromium carbides. 3V is only small vanadium carbides.

CPM-3V became Crucible’s go-to steel for applications requiring high toughness; they released it around 1999. Surprisingly this steel didn’t really take off in knives. And I would argue it never really has. Jerry Hossom was the first custom knifemaker I noticed using it regularly. In more recent years perhaps the best known user of the steel is Nathan Carothers with his “Delta” heat treatment. I don’t mean to suggest no one is using 3V, I see currently available knives from a range of manufacturers including Bark River, ESEE, Cold Steel, and others, but it never seems like there are as many 3V knives as there could be. I think it being non-stainless has held it back as knife manufacturers tend to stick with stainless steels.

Heat Treating and Hardness

I did a new set of heat treating coupons for CPM-3V as I wanted to go a bit higher on austenitizing temperature than coupons I had done for the book Knife Engineering. The hold time at 1850°F was 45 minutes, 1950°F was 30 minutes, 2050°F was 20 minutes, and 2150°F was 10 minutes. While CPM-3V is typically heat treated in the 58-62 Rc range because of its excellent toughness, it can be heat treated to higher hardness if desired. This is significantly higher than the 61 Rc the datasheet shows the steel maxing out at. This is because I used the low temper range (300-500°F), rather than the datasheet recommended high temper range (1000-1050°F).

Microstructure

CPM-3V has about 5% vanadium carbide, and is free of chromium carbide despite the relatively high chromium content. This is in contrast to Z-Tuff which has about 3% chromium carbide and only 1% vanadium carbide. CPM-1V also has about 1% vanadium carbide but about 2% M6C (molybdenum/tungsten carbides found in high speed steels). So 3V has only a bit higher carbide volume than those two steels but it is all the hard vanadium carbide type which should mean more balanced properties.

3V (1925°F) – 5% carbide volume

Z-Tuff (1925°F) = 4% carbide volume

CPM-1V (2050°F) – 3% carbide volume

Toughness

One mystery about CPM-3V toughness comes from a patented Crucible steel that was never released commercially, a modified version of 3V. The steel was patented in 2006 by Alojz Kajinin and Andrzej Wojciesczynski. I actually wrote about this modified steel in my very first article on Knife Steel Nerds in February 2018. I didn’t even advertise the article because it was a test before I wrote a series on austenitizing that I did promote with the announcement of the website. The modified 3V was designed by partially replacing vanadium with niobium, which made the carbides smaller. They showed experiments in the patent that the longitudinal toughness of 3V was much higher than the transverse toughness. With transverse toughness the crack grows along the rolling direction, and carbides and impurities are aligned along the rolling direction giving easier paths for crack growth. However, with the modified 3V they found the transverse toughness to be roughly equal to the longitudinal toughness.

So for a new experiment on CPM-3V I decided to test both the longitudinal and transverse toughness and see if the transverse toughness was really as bad as it was shown in the 3V mod patent. I used an austenitizing temperature of 2000°F, plate quench, cryo, and a temper at 400°F. This resulted in about 61.5 Rc, which is significantly higher in hardness than our original 3V toughness tests. Those coupons were heat treated by Warren Krywko who heat treated a whole bunch of toughness coupons that I tested early on. I think maybe the cooling rate in quenching he was performing was somewhat slower than what I did, maybe because he was doing many specimens at the same time in the plate quench. That is significant because a slower cooling rate leads to both lower hardness and lower toughness, as I wrote about in last month’s article. All of the coupons we heat treated were tempered at 400°F rather than the 1000°F temper the datasheet recommends, because of our earlier findings with CPM-CruWear/Z-Wear.

Comparing the hardness-toughness to the previous CPM-3V tests I found significantly better properties. The transverse toughness I measured was only ~7% worse than the longitudinal, which is quite impressive. The transverse toughness reported in the 3V mod patent looks like an anomaly, I have never seen such a large difference between longitudinal and transverse toughness. Though I have to say, the very small drop between longitudinal and transverse toughness I measured here is quite impressive.

With the improved toughness measurements 3V nearly rivals the results of Z-Tuff and CPM-1V which both have lower carbon and vanadium. This actually does make some sense, as the carbide volume is similar between the three steels. To me the composition designs of Z-Tuff and CPM-1V are not totally optimal because they have a significant amount of non-vanadium carbides. The best toughness-wear resistance balance is generally achieved by having all vanadium carbides. Perhaps in the future we could explore higher hardness heat treatments like in the 62-64 Rc range.

Wear Resistance and Edge Retention

I tested the CATRA edge retention of 3V way back in my giant CATRA study. It did exceptionally well for its level of toughness at 463 mm cardstock cut, significantly higher than CPM-1V and CD1/Z-Tuff. Looking back I do think the heat treatment used was cheating a bit, as the tempering temperature was only 300°F. If the tempering temperature was a more appropriate 400°F, the austenitizing temperature for the same hardness would be higher and thus there would be a bit less carbide in the steel. However, this would only marginally affect the final result.

Edge Retention-Toughness Balance

The combination of wear resistance and toughness of 3V is quite impressive. I added a new datapoint for 3V with its newly higher toughness test. I had to adjust up the CATRA edge retention based on the predicted change with hardness for the chart since the CATRA knife was 1.4 Rc lower than the toughness coupon. CPM-3V is really in a class of its own for the level of toughness it has for the level of edge retention. Of course it doesn’t do anything too crazy when it comes to edge retention, but it is sufficient for many knives and has excellent toughness to go with it.

Corrosion Resistance

I have never tested the corrosion resistance of CPM-3V. With its 7.5% Cr and no chromium carbide its corrosion resistance can be quite good for a non-stainless. Some people talk about “semi-stainless” steels and if any steel were to fit in this category it would be 3V. It actually has more chromium in solution than D2, which is perhaps the best known “semi-stainless” steel. Z-Tuff and CD#1 also have a similar chromium content but because they have some chromium carbide in the heat treated condition we would expect 3V to have somewhat better corrosion resistance. In a corrosion test performed by Scott Larimore and Kelly W., CPM-3V was found to survive “in the elements” without rust. However, this was only the case with the low temper condition (<750°F) but not the high temper condition (>750°F). This is expected, though the stark difference never fails to surprise me. The low temper condition is labeled “3VL” and the high temper condition is labeled “3VH.”

Corrosion test by Scott Larimore and Kelly W.

Summary and Conclusions

I think CPM-3V has an excellent set of properties with very high toughness and decent wear resistance and edge retention for that level of toughness. With the 7.5% Cr and lack of chromium carbides its level of corrosion resistance is also quite good for a non-stainless steel. I don’t see anyone out there criticizing the steel, but somehow it seems to never quite get the recognition and popularity it probably deserves.


[1] Johnstin, Harry G. “Alloy steels and articles thereof.” U.S. Patent 3,219,442, issued November 23, 1965.

[2] Pinnow, Kenneth E., and William Stasko. “Wear resistant, powder metallurgy cold work tool steel articles having high impact toughness and a method for producing the same.” U.S. Patent 5,830,287, issued November 3, 1998.

The post CPM-3V – Still the Best High Toughness Steel appeared first on Knife Steel Nerds.

  •  

Is 1084-15N20 the Best Pattern Welded Damascus?

Patreon

Several new experiments were done to support this article. I am able to do these experiments thanks to the contributions of Patreon supporters. If you would like to support knife steel research visit Patreon.com/KnifeSteelNerds

YouTube Video

Here is the video version of the following information:

Stainless and San-Mai

This article got too long so I will be discussing stainless steels, high alloy steels, and San-Mai laminates in a future article.

Historical Steel Combinations

I have a book on the history of steel in knives in “modern” times called The Story of Knife Steel: Innovators Behind Modern Damascus and Super Steels. I have a very short summary below of some of the content in that book but if you want to learn more about steel combinations and patterning in Damascus, you should read the book.

Early Bill Moran pattern-welded Damascus used O1 and mild steel. Moran and other 1970s and 1980s-era Damascus smiths believed that a large carbon difference would lead to the difference in etching behavior to provide a contrast. Dr. John Verhoeven and bladesmith Howard Clark in 1998 did a study on pattern-welded Damascus [1] where they found that carbon would diffuse evenly between two steels and thus have the same carbon content throughout. Instead they found that other alloying elements led to contrast after etching. Carbon is a very small element which is “interstitial,” meaning it sits between iron atoms. Larger elements like manganese, chromium, and nickel are “substitutional” atoms that replace iron atoms and thus diffusion is much slower.

Before the study by Verhoeven and Clark, Damascus smiths had already moved on to other combinations. Instead of mild steel a high nickel, low carbon steel A203E became popular for the “bright” layer in Damascus. This recommendation was made in 1977 [2] by the “Damascus Steel Research Team” of Daryl Meier, Jim Wallace, and Robert Griffith. They also recommended pure nickel metal as a bright layer. Anciently, nickel steel was used in some blades from metallic meteorites, which typically have 5-10% nickel. Early “dark” layer choices in the 1970s and 1980s were typically simple high carbon steels such as W1, W2, and 1095. Along with low alloy high carbon tool steels like O1 and O2.

A203E has only 0.1% carbon and there was an increasing desire by bladesmiths to use two high carbon steels for better hardness and wear resistance. Tim Zowada began using O2 and L6 high carbon steels from Carpenter around 1990-1991. It became increasingly common to use bandsaw blades which were typically made with high nickel steels such as 15N20. However, it was more common at that time to call this material “L6,” despite the fact that L6 has never been used in bandsaw blades as far as I can find. L6 is somewhat similar because it has 1.5% Ni but it is different than bandsaw blade steels.

Popularization of 1084 and 15N20

The steel combination of 1084 and 15N20 has become ubiquitous, though it did not become popular until the mid-to-late 1990s. For example, the Jim Hrisoulas book The Pattern Welded Blade from 1994 does not even mention 15N20, and he mostly wrote in that book about combining high carbon and low carbon steels. The 1084/15N20 combination was popularized in part by the “Montana Mafia,” made up of Damascus smiths such as Rick Dunkerley and Shane Taylor. Dunkerley reported that he began using this mix in 1995 from a suggestion from Devin Thomas [3]. I asked my father Devin why he suggested these steels and he said that a lot of bladesmiths would ask him for help with forge welding and etching issues but a lot of people were using difficult steel combinations. He felt that 1084 and 15N20 were easy to forge weld and would give a good contrast.

15N20 has 0.75% carbon along with 2% nickel, so like other nickel alloyed steels it can act as the “bright” layer in Damascus. 1084 has only slightly higher carbon at 0.84% and has elevated manganese when compared with 1095 (0.75 vs 0.4% Mn). 1075 has the same 0.75% carbon of 15N20 so I also asked my father why it was 1084 and not 1075. He said that 1075 was typically available as wide sheet which would require shearing down to narrow pieces for the billet. 1084 was available as narrower “bar” which could be bandsaw cut for the stack with 15N20. For some knifemakers it was appealing that 1084 had more carbon than 1075. Regardless, 1075, 1080, and 1084 are roughly equivalent.

Rick Dunkerley folder in 1084 and 15N20

Etching Response

Notes on Comparisons

Comparing etching response of different combinations can be somewhat tricky because of a few factors:

  1. Different etchants may lead to different levels of contrast
  2. Etching and polishing technique affect contrast
  3. Photography has a big effect on contrast. You may have experienced times when you saw a Damascus knife in an image with very clear contrast but once in person you see it is much more subtle.

So despite those difficulties I am going to make some generalizations about level of contrast with different combinations. If you disagree with my assessment feel free to say so in the comments.

Nickel

It has long been understood that the nickel content in steels like 15N20 allows them to resist etching and thus provide the “bright” layer in Damascus. However, when you etch 15N20 on its own it etches dark just fine so I think it may be some kind of anode/cathode effect at work where the 1084 is etched preferentially rather than the 15N20 resisting etching on its own. Higher nickel seems to lead to greater contrast than lower nickel, so 15N20 with its 2% nickel does pretty well. There are some rarer steels with 4% nickel, such as 4800 steel powder or Bohler K600 (1.2767). L6 has somewhat lower nickel at 1.5% and 8670 even lower with ~0.9%. Unfortunately there aren’t any low alloy nickel steels with significant vanadium or tungsten additions so wear resistance typically needs to come from the other steel used in the combination.

Nickel knife steels. Note: I found conflicting information on 4600 and 4800 compositions so I left the Mn blank. Some list there being 0.5% Mo. The most common versions have little or no carbon, and the “KC” versions have carbon added to them, usually graphite. I have also heard that some distributors take 1080 powder and add nickel powder.

Manganese (and Carbon)

Higher manganese leads to darker etching. For example, in the Verhoeven/Clark study they found that with 1018 (0.75% Mn) and 1086 steel (0.4% Mn) the 1018 was the “dark” layer despite its lower carbon content. This demonstrates that the old view that carbon differences led to etching contrast was incorrect.

Image from [1]. Notice the higher carbon steel is the “light” layer.

The higher Mn in 1084 relative to 1095 and 1075 leads to it being somewhat darker when in combination with 15N20. Some steels with even higher Mn etch even darker such as O1 (1.2%) and O2 (1.6%). The European version of O2 called 1.2842 has 2% Mn and etches darker than perhaps any other common steel.

Chromium

Chromium is a bit more mysterious as to its effects. In the Verhoeven/Clark study they found that 52100/L6 had poor contrast. 52100 has high chromium (1.5%) but also low manganese (0.35%). I have seen knives here or there with 52100 and 15N20 and the contrast can be “ok” in some of them, such as this feather pattern bowie by Aaron Wilburn:

Aaron Wilburn feather Damascus in 52100 and 15N20

1095 steel has similar carbon content to 52100 and slightly more Mn (0.45%) but without chromium. It typically etches darker than 52100 when in combination with 15N20, as seen in this knife:

Blake Nichols knife with Greg Shahan Damascus in 1095 and 15N20

O1 still etches quite dark despite having 0.5% Cr and so does 1.2842 despite having 0.35% Cr. 80CrV2 is also generally considered sufficiently dark in combination with 15N20 even though it has 0.5% Cr and only 0.4% Mn. 5160 has relatively high Mn (~0.85%) and Cr (0.8%) and it can also etch relatively dark despite the Cr addition.

So I think overall it appears that low amounts of Cr do not have a large effect on etching response, but higher amounts like the 1.5% in 52100 may affect how dark steel etches.

Vanadium, Tungsten, Molybdenum

As far as I can tell these elements do not effect etching. However, high vanadium and/or tungsten additions are good for higher wear resistance and edge retention in Damascus so I have included the composition of several of them below:

“3-color Damascus”

Sometimes steel combinations can be used that give multiple shades of grey/white. A common example would be a dark etching steel in combination with 15N20 and pure nickel. While 15N20 does resist etching it doesn’t do so nearly to the extent of pure nickel so three different shades are achieved.

Sometimes an intermediate shade steel can be found between 15N20 and a dark etching steel. One example I found was 1.2842/80CrV2/15N20 Damascus [4]. There can also be some contrast between 2% Ni 4600 and 4% Ni 4800 as seen comparing the eyes (4800) and beak (4600) in the roadrunner by Cliff Parker below:

Cliff Parker Damascus roadrunner. Bright lines are nickel sheet, eyes are 4800, beak is 4600, and the rest is 1084/1018 mixed.

Forge Welding Temperatures – Crumbling, Melting

It is quite common for Damascus smiths to use very high forge welding temperatures such as 2300, 2350°F (1260-1290°C) or sometimes even hotter. This typically works for steels like 1084 and 15N20. However, with higher carbon the melting temperature of the steel is reduced. The grain boundaries melt first. After the grain boundaries melt the steel will crumble during forging. This is especially important to keep in mind when steels have higher than 1.2% carbon like 26C3, ApexUltra, 1.2562, Blue Super, White #1, etc. However, even 1% carbon steels like W1 and 52100 can cause problems for Damascus smiths that are used to pushing the temperature as much as possible with lower carbon mixes like 1084 and 15N20. With these very high carbon steels, a reduced temperature is likely necessary such as 2150-2200°F (1175-1205°C). A longer soak time can make up for reduced forge welding temperatures.

Ease in Forging

I have a separate article on difficulty in forging of different steels. I have a loose ranking of some typical steels in terms of difficulty in forging in that article. Typically, higher carbon and higher alloy steels are more difficult to forge. One reason is because those steels are more likely to have undissolved carbides at the forging temperature. Those carbides don’t deform as well as steel which increases the difficulty.

Steels below the eutectoid (~0.77% carbon) are very easy to dissolve the carbides. The carbides would likely be dissolved well below the forge welding temperature. Steels with very high carbon like 26C3 (1.25% C) may still have some carbide near the forging temperature. 52100, even though it only has 1% carbon, also has 1.5% chromium which raises the temperature at which carbides dissolve. However, even 26C3 and 52100 will have very little carbide when compared to something like D2, and the remaining carbides would be much smaller. Some low alloy steels have vanadium and tungsten additions for greater wear resistance like CruForgeV and ApexUltra. Those vanadium and tungsten carbides are still present at forging temperatures and can affect forgeability.

How Well Do They “Stick”?

When forge welding in an oxygen atmosphere, oxides form on the surface which prevents diffusion bonding. Flux dissolves the oxides, allowing the two pieces of steel to bond. Some alloying elements will change the type of oxide that will form. The most common example is chromium in stainless steels, which famously cannot be forge welded with the conventional flux method. The chromium oxides are not dissolved by flux and therefore forge welding is not typically possible. Manganese and nickel do not seem to have a large effect which is why 1084 and 15N20 are easily forge welded using flux. The higher the chromium content, the more difficult the steel is to be forge welded. However, if the steel is in an oxygen-free environment then difficult steels can still be forge welded.

Cracking After Forging

High hardenability steels can partially harden after forging and this can lead to cracking, sometimes several hours later. Oil hardening steels like O1, O2, and L6 are more sensitive to this behavior. It helps to slow cool from below a certain temperature (like 1400°F/760°C or so). Slow cooling from very high temperatures can lead to carbides forming on the grain boundaries that are difficult to eliminate. Low alloy steels can be normalized to dissolve the carbides though air hardening steels cannot be normalized. After cooling to room temperature (whether slowly on purpose or unintentionally quickly), the steel can by cycled or annealed to remove the stresses in the material so that cracking doesn’t happen.

Austenitizing

Hardness

Semi-frequently I get questions from knife enthusiasts (and even some Damascus smiths) about combining non-typical steels together. Sometimes bizarre combinations like MagnaCut and 15N20. Often times the reason these steels are not compatible is because of the austenitizing (hardening) temperature range. 15N20 is optimally austenitized from about 1400-1475°F (760-800°C), while MagnaCut is austenitized from 1950-2200°F (1065-1205°C). As you can see, these two ranges do not overlap. If the MagnaCut was austenitized from 1475°F it would be very soft (and corrosion resistance would be lower than 1950+ as well). If the 15N20 was austenitized at 1950°F or higher it would have very poor toughness from grain growth. Some steels can be pushed a bit higher or lower than typically recommended in a datasheet but this is obviously not an example of where that can happen.

MagnaCut and 15N20 is of course an extreme example but austenitizing ranges can also be relevant even with low alloy non-stainless steels. For example, Mn and Ni push down the temperature at which steel transforms to austenite, and Cr increases the temperature where steel transforms to austenite. You can see this in the chart below where I austenitized steel in 25°F increments and quenched in oil (from a normalized microstructure).

You can see that 15N20 with the 2% Ni addition is fully austenitized (from a normalized, pearlite microstructure) from 1325°F (720°C) while 1084 was still dead soft after quenching from that temperature. The 1084 instead showed full hardness at 1350°F (732°C), only 25°F hotter. 80CrV2 has 0.5% Cr, however, which increases the temperature at which carbide dissolves, and full as-quenched hardness was not achieved until about 1400°F (760°C). This is from a normalized microstructure, not an annealed microstructure. The annealing procedure can have a large effect on heat treating behavior. Below is a chart of 80CrV2 after austenitizing from different temperatures:

As you can see, there is a significant difference between a pearlitic starting microstructure (normalized) and annealed. And in this case even a sizeable difference in the annealed microstructure of the two different suppliers. The Cr addition makes the starting microstructure have a particularly large effect on the heat treating response. This is why Cr alloyed steels often have a somewhat higher recommended austenitizing temperature than Cr-free steels such as 1500-1550°F (815-845°C).

15N20, only alloyed with Mn and Ni, shows a much smaller effect of starting microstructure on heat treating response:

The “Fast DET” anneal was my own annealing procedure with a faster cooling rate. The “Steel company anneal” is the steel as it was received from the manufacturer. You can see that with the steel as-received the peak hardness is not achieved until about 1400°F which is ~75°F higher than a normalized microstructure. But 1400°F is a much lower temperature than was necessary for factory annealed 80CrV2. This helps explain why Cr-free steels are usually austenitized from a somewhat lower temperature such as 1475°F (800°C).

Toughness – Grain Growth

However, there is also an upper end of acceptable temperature, which is where grain growth occurs. For chromium-alloyed steel, toughness typically peaks around 1500-1550°F (815-845°C) and drops from there. This was found with 5160, 52100, and 8670, for example. Carbides can “pin” grain boundaries and prevent grain growth. Because chromium stabilizes the carbides to higher temperatures, grain growth does not occur until somewhat higher temperatures than steels alloyed only with Mn and Ni. Vanadium can extend this temperature range further, as the vanadium carbides do not dissolve until higher temperatures. This is why small vanadium additions (~0.2%) are made to certain steels like W2 and 80CrV2. In my tests of 80CrV2, toughness had not dropped even with an austenitizing temperature of 1580°F (860°C), though I did not try any higher. But 15N20 does not have any chromium or vanadium so we did a new series of tests with 15N20. We also added two other steels, L6, a 1.5% Ni steel with a chromium addition; and 1.2519, a steel with chromium, tungsten, and vanadium (all three of those elements can help prevent grain growth). Each of them were heat treated from the annealed condition as-received from the steel manufacturer.

In terms of hardness, the steels behave in ways I have been describing. The L6 and 1.2519 increased in hardness with higher austenitizing temperature. This is because the steels were alloyed with chromium, delaying the dissolution of carbides. 15N20, lacking chromium, was flat in hardness between 1400 and 1600°F.

The L6 peaked in toughness at 1500°F which is similar to other chromium-alloyed steels. The toughness actually increased between 1400 (760°C) and 1500°F (815°C), which is because we are dissolving some carbide (carbides are brittle),  but not getting too much carbon in solution or grain growth. So the optimal austenitizing temperature for L6 would be around 1500°F, as that gives us a good combination of hardness and toughness. 1.2519 had flat toughness between 1400 and 1500°F though hardness also increased significantly over that range. Therefore, the hardness-toughness balance peaked at 1500°F even though the toughness did not change between 1400 and 1500°F. Toughness dropped slightly at 1550-1600°F (845-870°C), which is either due to grain growth or perhaps too much carbon in solution (I will explain that next).

With 15N20, the toughness dropped significantly even with 1500°F. In an earlier test with 15N20 I also found good toughness from 1475°F (800°C). So grain growth and a drop in toughness was found even with 1500°F, the same temperature that gave the peak properties for L6! I was surprised that toughness dropped off so rapidly for 15N20 at 1500°F, which I did not think sufficiently high to cause significant problems, even in a steel with little carbide like 15N20. This may have affected the toughness results of two 15N20 combinations I tested in my prior study, one with 1.2419 and the other with CruForgeV. 1084 is also very sensitive to overheating, grain growth, and a reduction in toughness. So despite how easy it is for 1084 and 15N20 to be hardened, I recommend using a furnace to avoid grain growth and a toughness drop.

80CrV2 and 15N20

So 15N20 needs to be austenitized at 1475°F (800°C) or below to avoid poor toughness, but 80CrV2 is more optimal from 1500-1525°F (815-830°C). Perhaps L6 is the more optimal steel to combine with 80CrV2, and 15N20 is more optimal to be used with 1084. However, the 80CrV2 can be processed to be more compatible with the 15N20. If starting from a normalized microstructure, the steel can be austenitized from a lower temperature to match the 15N20. Normalized steel is somewhat harder, and therefore more difficult to drill and bandsaw cut. With normalized 80CrV2 I found it to be about 25 Rc. This value can vary some based on the cooling rate (greatly affected by the size of the piece). If another grain refining step was added by heating to 1400°F (760°C) and air cooling, the hardness is dropped to about 19 Rc without significantly affecting the hardening response. Generally I prefer to use a “Fast DET” anneal before austenitizing instead, but this is one of the exceptions to that general recommendation.

Toughness – Carbon in Solution and Plate Martensite

Grain growth is not the only source of reduced toughness with higher austenitizing temperatures. The higher you austenitize, the more carbide is dissolved, putting more carbon “in solution,” which is why hardness is increased with temperature. However, as carbon in solution increases past 0.6% you get more “plate martensite” which is brittle and reduces toughness. You can read more about plate martensite in this article. With a steel like 15N20, the carbon content is only 0.75%, so this is not as much of an issue. However, when steels have over 0.85% carbon, they are more in danger of low toughness from plate martensite. Below is the example of O1 steel, austenitized from 1425 (775°C), 1475 (800°C), and 1550°F (845°C). Despite 1475°F not being hot enough for grain growth in O1, there was a significant reduction in toughness by austenitizing at 1475 instead of 1425°F. This was further reduced by austenitizing at 1550°F. So this is yet another reason to pay attention to optimal austenitizing ranges for different steels before combining them in pattern-welded Damascus.

Normalizing and Annealing

I know it seems slightly out of order to talk normalizing and annealing after austenitizing (to quench), but we are typically austenitizing the steel to perform these two steps as well. Compensating for normalizing is not too difficult with various Damascus combinations. It is generally best to take the higher required normalizing temperature of the two. For example, if you had combined 26C3, which needs something like 1700°F (925°C) to normalize, and combined it with 15N20 which only needs 1550°F (845°C) or so, you would normalize at 1700°F. The temperature needs to be sufficiently high to dissolve all the carbides, and the 1550°F for 15N20 would not be sufficiently high for the 26C3.

For annealing, similar rules apply. You generally want to use the higher required annealing temperature to ensure that both are annealed. If too much carbide is dissolved in one of the steels, that can mean you get pearlite at the end instead of spheroidized carbide and thus a little higher annealed hardness. But that is usually an acceptable tradeoff. As I mentioned in the 80CrV2/15N20 section, for some combinations a pearlitic, normalized structure may make the steels more compatible in heat treatment. In this case you would normalize like normal at the required temperature for 80CrV2 (1550-1650°F). Then heat to the annealing temperature for 80CrV2 (1400°F), but instead of slow cooling do air cooling. This is a grain refinement cycle instead of annealing. Normally grain refinement cycles aren’t necessary when annealing because the low temperature anneal also refines the grain. Generally I prefer annealed steel outside of specific cases such as mixing chromium and non-chromium steels. Or steel that will be heat treated in an uncontrolled forge.

I have a separate article on normalizing and annealing with recommended procedures and temperatures.

Quenching and Hardenability

Steels also have different levels of “hardenability,” or how fast they need to be quenched to be fully hardened. For example, there are “water hardening,” “oil hardening,” and “air hardening” steels. Even within low alloy non-stainless steels there can be significant differences. For example, L6 is a high hardenability oil hardening steel, while W2 is a very low hardenability water hardening steel. The two can be used together, but there is a significant gap between the two steels for hardenability. This means that to fully harden the W2/L6 Damascus you need to quench very rapidly for the W2 to ensure it fully hardens. If a slow oil was used you would likely end up with hardened L6 but soft W2. Even 1084 and 15N20 have a difference in hardenability because the 2% Ni addition in the 15N20 means its hardenability is higher despite the lower Mn. I have a loose ranking of hardenability of different steels in this article.

Tempering

Tempering leads to darker etching than untempered steel [1]. Some people using Damascus for decorative purposes (thus not needing high hardness) will skip the heat treatment but this leads to poorer contrast. Martensite etches better than ferrite, and tempered martensite etches even better.

In terms of compatibility, tempering is usually not a big deal. Most steels can be tempered at ~400°F and achieve good properties. Some steels have a slightly different range than others. 15N20 and 8670 needed to be tempered at least at 350°F for achieving high toughness and 5160 needed 375°F. The steels were not necessarily brittle below those temperatures, but did not have the high toughness the steels are known for.

You can also see that the toughness of 15N20 dropped when tempering at 450°F, which is called “Tempered Martensite Embrittlement.” The temperature at which TME is first seen changes some by steel, and some do not see the phenomena until 500°F or even higher. However, 400°F is safe for any steel I have so far tested.

Toughness and Edge Retention

I already have a whole article on the testing of toughness and edge retention of pattern-welded Damascus so I won’t rehash all of that here. But there are a few key points to mention here when it comes to compatibility:

  1. Combining a low toughness and high toughness steel generally seems to lead to toughness similar to the low toughness steel. It fractures at the “weakest link” and there isn’t much benefit to adding a high toughness steel in terms of overall toughness.
  2. High wear resistance steels with high slicing edge retention generally still cut very well even when combined with a steel with lower wear resistance. So combining CruForgeV and 15N20 or ApexUltra and L6 led to edge retention similar to CruForgeV or ApexUltra. However, this was due in part to the improvement in edge retention seen in ladder patterning.
  3. While ladder patterning benefited edge retention it also slightly reduced toughness.
  4. A “Damascus Cutting Effect” was seen in a 1095/Nickel Damascus. Most steel combinations do not have hard and soft layers but using nickel does provide this potential benefit.

When not attempting to have the “Damascus Cutting Effect” it can be beneficial to have two steels with good wear resistance. For low alloy non-stainless steels it makes sense to look at steels with significant vanadium and/or tungsten additions like ApexUltra, CruForgeV, 1.2519, 1.2419, 1.2562, Blue Super, V-Toku1, etc. However, for low alloy steels the main choices for a “bright” layer are 15N20 and L6 and neither has much wear resistance.

If making a Damascus combination for high toughness there must be two high toughness steels. 1084 and 15N20 are a decent combination for this. 1084 is somewhat lower in toughness but the two together still tested at ~34 ft-lbs in a random pattern (as opposed to 45-50 ft-lbs for 15N20).

Summary and Conclusions

It is best to choose steels that have similar temperatures for heat treating. High manganese is best for a dark layer after etching while Nickel is best for a bright layer. Other alloying elements can make forge welding difficult when using conventional flux methods, especially high levels of chromium. It is important to adjust heat treatment based on the steels that are combined together. For example, 15N20 sees a large toughness drop when austenitized at 1500°F. So when 1084 and 15N20 are used together it is best to heat treat with a furnace so that the steel isn’t overheated. The optimal temperature range for austenitizing 80CrV2 is too high for 15N20. If 80CrV2 and 15N20 are used together it is better to use a normalized starting structure so that a lower austenitizing temperature of 1475°F (800°C) can be used with the 80CrV2 and still achieve high hardness. L6 may be more optimal than 15N20 to use along with other chromium-alloyed steels though it has lower nickel than 15N20 (thus contrast is not as good), and is also more difficult to work with because of its alloy additions. High carbon steels are more sensitive to overheating because the grain boundaries melt, leading to crumbling during forging. High vanadium and tungsten steels are best for high wear resistance combinations, though they typically need to be combined with 15N20 or L6 which unfortunately do not have much wear resistance.


[1] Verhoeven, John D., and Howard F. Clark. “Carbon diffusion between the layers in modern pattern-welded Damascus blades.” Materials characterization 41, no. 5 (1998): 183-191.

[2] Meilach, Dona Z., George Martin, E. A. Chase, and Theodore Davidson. “Decorative and sculptural ironwork: tools, techniques, inspiration.” 1977.

[3] Dunkerley, Rick. “His Forge Burns Hot for Mosaic Damascus.” Kertzman, Joe, ed. Blade’s Guide to Making Knives. Krause Publications, 2005.

[4] https://www.kovares.com/product-page/165mm-damascus-petty

 

The post Is 1084-15N20 the Best Pattern Welded Damascus? appeared first on Knife Steel Nerds.

  •  

Is 1084-15N20 The Best? Pattern-Welded Damascus

Patreon

Several new experiments were done to support this article. I am able to do these experiments thanks to the contributions of Patreon supporters. If you would like to support knife steel research visit Patreon.com/KnifeSteelNerds

YouTube Video

Here is the video version of the following information:

Stainless and San-Mai

This article got too long so I will be discussing stainless steels, high alloy steels, and San-Mai laminates in a future article.

Historical Steel Combinations

I have a book on the history of steel in knives in “modern” times called The Story of Knife Steel: Innovators Behind Modern Damascus and Super Steels. I have a very short summary below of some of the content in that book but if you want to learn more about steel combinations and patterning in Damascus, you should read the book.

Early Bill Moran pattern-welded Damascus used O1 and mild steel. Moran and other 1970s and 1980s-era Damascus smiths believed that a large carbon difference would lead to the difference in etching behavior to provide a contrast. Dr. John Verhoeven and bladesmith Howard Clark in 1998 did a study on pattern-welded Damascus [1] where they found that carbon would diffuse evenly between two steels and thus have the same carbon content throughout. Instead they found that other alloying elements led to contrast after etching. Carbon is a very small element which is “interstitial,” meaning it sits between iron atoms. Larger elements like manganese, chromium, and nickel are “substitutional” atoms that replace iron atoms and thus diffusion is much slower.

Before the study by Verhoeven and Clark, Damascus smiths had already moved on to other combinations. Instead of mild steel a high nickel, low carbon steel A203E became popular for the “bright” layer in Damascus. This recommendation was made in 1977 [2] by the “Damascus Steel Research Team” of Daryl Meier, Jim Wallace, and Robert Griffith. They also recommended pure nickel metal as a bright layer. Anciently, nickel steel was used in some blades from metallic meteorites, which typically have 5-10% nickel. Early “dark” layer choices in the 1970s and 1980s were typically simple high carbon steels such as W1, W2, and 1095. Along with low alloy high carbon tool steels like O1 and O2.

A203E has only 0.1% carbon and there was an increasing desire by bladesmiths to use two high carbon steels for better hardness and wear resistance. Tim Zowada began using O2 and L6 high carbon steels from Carpenter around 1990-1991. It became increasingly common to use bandsaw blades which were typically made with high nickel steels such as 15N20. However, it was more common at that time to call this material “L6,” despite the fact that L6 has never been used in bandsaw blades as far as I can find. L6 is somewhat similar because it has 1.5% Ni but it is different than bandsaw blade steels.

Popularization of 1084 and 15N20

The steel combination of 1084 and 15N20 has become ubiquitous, though it did not become popular until the mid-to-late 1990s. For example, the Jim Hrisoulas book The Pattern Welded Blade from 1994 does not even mention 15N20, and he mostly wrote in that book about combining high carbon and low carbon steels. The 1084/15N20 combination was popularized in part by the “Montana Mafia,” made up of Damascus smiths such as Rick Dunkerley and Shane Taylor. Dunkerley reported that he began using this mix in 1995 from a suggestion from Devin Thomas [3]. I asked my father Devin why he suggested these steels and he said that a lot of bladesmiths would ask him for help with forge welding and etching issues but a lot of people were using difficult steel combinations. He felt that 1084 and 15N20 were easy to forge weld and would give a good contrast.

15N20 has 0.75% carbon along with 2% nickel, so like other nickel alloyed steels it can act as the “bright” layer in Damascus. 1084 has only slightly higher carbon at 0.84% and has elevated manganese when compared with 1095 (0.75 vs 0.4% Mn). 1075 has the same 0.75% carbon of 15N20 so I also asked my father why it was 1084 and not 1075. He said that 1075 was typically available as wide sheet which would require shearing down to narrow pieces for the billet. 1084 was available as narrower “bar” which could be bandsaw cut for the stack with 15N20. For some knifemakers it was appealing that 1084 had more carbon than 1075. Regardless, 1075, 1080, and 1084 are roughly equivalent.

Rick Dunkerley folder in 1084 and 15N20

Etching Response

Notes on Comparisons

Comparing etching response of different combinations can be somewhat tricky because of a few factors:

  1. Different etchants may lead to different levels of contrast
  2. Etching and polishing technique affect contrast
  3. Photography has a big effect on contrast. You may have experienced times when you saw a Damascus knife in an image with very clear contrast but once in person you see it is much more subtle.

So despite those difficulties I am going to make some generalizations about level of contrast with different combinations. If you disagree with my assessment feel free to say so in the comments.

Nickel

It has long been understood that the nickel content in steels like 15N20 allows them to resist etching and thus provide the “bright” layer in Damascus. However, when you etch 15N20 on its own it etches dark just fine so I think it may be some kind of anode/cathode effect at work where the 1084 is etched preferentially rather than the 15N20 resisting etching on its own. Higher nickel seems to lead to greater contrast than lower nickel, so 15N20 with its 2% nickel does pretty well. There are some rarer steels with 4% nickel, such as 4800 steel powder or Bohler K600 (1.2767). L6 has somewhat lower nickel at 1.5% and 8670 even lower with ~0.9%. Unfortunately there aren’t any low alloy nickel steels with significant vanadium or tungsten additions so wear resistance typically needs to come from the other steel used in the combination.

Nickel knife steels. Note: I found conflicting information on 4600 and 4800 compositions so I left the Mn blank. Some list there being 0.5% Mo. The most common versions have little or no carbon, and the “KC” versions have carbon added to them, usually graphite. I have also heard that some distributors take 1080 powder and add nickel powder.

Manganese (and Carbon)

Higher manganese leads to darker etching. For example, in the Verhoeven/Clark study they found that with 1018 (0.75% Mn) and 1086 steel (0.4% Mn) the 1018 was the “dark” layer despite its lower carbon content. This demonstrates that the old view that carbon differences led to etching contrast was incorrect.

Image from [1]. Notice the higher carbon steel is the “light” layer.

The higher Mn in 1084 relative to 1095 and 1075 leads to it being somewhat darker when in combination with 15N20. Some steels with even higher Mn etch even darker such as O1 (1.2%) and O2 (1.6%). The European version of O2 called 1.2842 has 2% Mn and etches darker than perhaps any other common steel.

Chromium

Chromium is a bit more mysterious as to its effects. In the Verhoeven/Clark study they found that 52100/L6 had poor contrast. 52100 has high chromium (1.5%) but also low manganese (0.35%). I have seen knives here or there with 52100 and 15N20 and the contrast can be “ok” in some of them, such as this feather pattern bowie by Aaron Wilburn:

Aaron Wilburn feather Damascus in 52100 and 15N20

1095 steel has similar carbon content to 52100 and slightly more Mn (0.45%) but without chromium. It typically etches darker than 52100 when in combination with 15N20, as seen in this knife:

Blake Nichols knife with Greg Shahan Damascus in 1095 and 15N20

O1 still etches quite dark despite having 0.5% Cr and so does 1.2842 despite having 0.35% Cr. 80CrV2 is also generally considered sufficiently dark in combination with 15N20 even though it has 0.5% Cr and only 0.4% Mn. 5160 has relatively high Mn (~0.85%) and Cr (0.8%) and it can also etch relatively dark despite the Cr addition.

So I think overall it appears that low amounts of Cr do not have a large effect on etching response, but higher amounts like the 1.5% in 52100 may affect how dark steel etches.

Vanadium, Tungsten, Molybdenum

As far as I can tell these elements do not effect etching. However, high vanadium and/or tungsten additions are good for higher wear resistance and edge retention in Damascus so I have included the composition of several of them below:

“3-color Damascus”

Sometimes steel combinations can be used that give multiple shades of grey/white. A common example would be a dark etching steel in combination with 15N20 and pure nickel. While 15N20 does resist etching it doesn’t do so nearly to the extent of pure nickel so three different shades are achieved.

Sometimes an intermediate shade steel can be found between 15N20 and a dark etching steel. One example I found was 1.2842/80CrV2/15N20 Damascus [4]. There can also be some contrast between 2% Ni 4600 and 4% Ni 4800 as seen comparing the eyes (4800) and beak (4600) in the roadrunner by Cliff Parker below:

Cliff Parker Damascus roadrunner. Bright lines are nickel sheet, eyes are 4800, beak is 4600, and the rest is 1084/1018 mixed.

Forge Welding Temperatures – Crumbling, Melting

It is quite common for Damascus smiths to use very high forge welding temperatures such as 2300, 2350°F (1260-1290°C) or sometimes even hotter. This typically works for steels like 1084 and 15N20. However, with higher carbon the melting temperature of the steel is reduced. The grain boundaries melt first. After the grain boundaries melt the steel will crumble during forging. This is especially important to keep in mind when steels have higher than 1.2% carbon like 26C3, ApexUltra, 1.2562, Blue Super, White #1, etc. However, even 1% carbon steels like W1 and 52100 can cause problems for Damascus smiths that are used to pushing the temperature as much as possible with lower carbon mixes like 1084 and 15N20. With these very high carbon steels, a reduced temperature is likely necessary such as 2150-2200°F (1175-1205°C). A longer soak time can make up for reduced forge welding temperatures.

Ease in Forging

I have a separate article on difficulty in forging of different steels. I have a loose ranking of some typical steels in terms of difficulty in forging in that article. Typically, higher carbon and higher alloy steels are more difficult to forge. One reason is because those steels are more likely to have undissolved carbides at the forging temperature. Those carbides don’t deform as well as steel which increases the difficulty.

Steels below the eutectoid (~0.77% carbon) are very easy to dissolve the carbides. The carbides would likely be dissolved well below the forge welding temperature. Steels with very high carbon like 26C3 (1.25% C) may still have some carbide near the forging temperature. 52100, even though it only has 1% carbon, also has 1.5% chromium which raises the temperature at which carbides dissolve. However, even 26C3 and 52100 will have very little carbide when compared to something like D2, and the remaining carbides would be much smaller. Some low alloy steels have vanadium and tungsten additions for greater wear resistance like CruForgeV and ApexUltra. Those vanadium and tungsten carbides are still present at forging temperatures and can affect forgeability.

How Well Do They “Stick”?

When forge welding in an oxygen atmosphere, oxides form on the surface which prevents diffusion bonding. Flux dissolves the oxides, allowing the two pieces of steel to bond. Some alloying elements will change the type of oxide that will form. The most common example is chromium in stainless steels, which famously cannot be forge welded with the conventional flux method. The chromium oxides are not dissolved by flux and therefore forge welding is not typically possible. Manganese and nickel do not seem to have a large effect which is why 1084 and 15N20 are easily forge welded using flux. The higher the chromium content, the more difficult the steel is to be forge welded. However, if the steel is in an oxygen-free environment then difficult steels can still be forge welded.

Cracking After Forging

High hardenability steels can partially harden after forging and this can lead to cracking, sometimes several hours later. Oil hardening steels like O1, O2, and L6 are more sensitive to this behavior. It helps to slow cool from below a certain temperature (like 1400°F/760°C or so). Slow cooling from very high temperatures can lead to carbides forming on the grain boundaries that are difficult to eliminate. Low alloy steels can be normalized to dissolve the carbides though air hardening steels cannot be normalized. After cooling to room temperature (whether slowly on purpose or unintentionally quickly), the steel can by cycled or annealed to remove the stresses in the material so that cracking doesn’t happen.

Austenitizing

Hardness

Semi-frequently I get questions from knife enthusiasts (and even some Damascus smiths) about combining non-typical steels together. Sometimes bizarre combinations like MagnaCut and 15N20. Often times the reason these steels are not compatible is because of the austenitizing (hardening) temperature range. 15N20 is optimally austenitized from about 1400-1475°F (760-800°C), while MagnaCut is austenitized from 1950-2200°F (1065-1205°C). As you can see, these two ranges do not overlap. If the MagnaCut was austenitized from 1475°F it would be very soft (and corrosion resistance would be lower than 1950+ as well). If the 15N20 was austenitized at 1950°F or higher it would have very poor toughness from grain growth. Some steels can be pushed a bit higher or lower than typically recommended in a datasheet but this is obviously not an example of where that can happen.

MagnaCut and 15N20 is of course an extreme example but austenitizing ranges can also be relevant even with low alloy non-stainless steels. For example, Mn and Ni push down the temperature at which steel transforms to austenite, and Cr increases the temperature where steel transforms to austenite. You can see this in the chart below where I austenitized steel in 25°F increments and quenched in oil (from a normalized microstructure).

You can see that 15N20 with the 2% Ni addition is fully austenitized (from a normalized, pearlite microstructure) from 1325°F (720°C) while 1084 was still dead soft after quenching from that temperature. The 1084 instead showed full hardness at 1350°F (732°C), only 25°F hotter. 80CrV2 has 0.5% Cr, however, which increases the temperature at which carbide dissolves, and full as-quenched hardness was not achieved until about 1400°F (760°C). This is from a normalized microstructure, not an annealed microstructure. The annealing procedure can have a large effect on heat treating behavior. Below is a chart of 80CrV2 after austenitizing from different temperatures:

As you can see, there is a significant difference between a pearlitic starting microstructure (normalized) and annealed. And in this case even a sizeable difference in the annealed microstructure of the two different suppliers. The Cr addition makes the starting microstructure have a particularly large effect on the heat treating response. This is why Cr alloyed steels often have a somewhat higher recommended austenitizing temperature than Cr-free steels such as 1500-1550°F (815-845°C).

15N20, only alloyed with Mn and Ni, shows a much smaller effect of starting microstructure on heat treating response:

The “Fast DET” anneal was my own annealing procedure with a faster cooling rate. The “Steel company anneal” is the steel as it was received from the manufacturer. You can see that with the steel as-received the peak hardness is not achieved until about 1400°F which is ~75°F higher than a normalized microstructure. But 1400°F is a much lower temperature than was necessary for factory annealed 80CrV2. This helps explain why Cr-free steels are usually austenitized from a somewhat lower temperature such as 1475°F (800°C).

Toughness – Grain Growth

However, there is also an upper end of acceptable temperature, which is where grain growth occurs. For chromium-alloyed steel, toughness typically peaks around 1500-1550°F (815-845°C) and drops from there. This was found with 5160, 52100, and 8670, for example. Carbides can “pin” grain boundaries and prevent grain growth. Because chromium stabilizes the carbides to higher temperatures, grain growth does not occur until somewhat higher temperatures than steels alloyed only with Mn and Ni. Vanadium can extend this temperature range further, as the vanadium carbides do not dissolve until higher temperatures. This is why small vanadium additions (~0.2%) are made to certain steels like W2 and 80CrV2. In my tests of 80CrV2, toughness had not dropped even with an austenitizing temperature of 1580°F (860°C), though I did not try any higher. But 15N20 does not have any chromium or vanadium so we did a new series of tests with 15N20. We also added two other steels, L6, a 1.5% Ni steel with a chromium addition; and 1.2519, a steel with chromium, tungsten, and vanadium (all three of those elements can help prevent grain growth). Each of them were heat treated from the annealed condition as-received from the steel manufacturer.

In terms of hardness, the steels behave in ways I have been describing. The L6 and 1.2519 increased in hardness with higher austenitizing temperature. This is because the steels were alloyed with chromium, delaying the dissolution of carbides. 15N20, lacking chromium, was flat in hardness between 1400 and 1600°F.

The L6 peaked in toughness at 1500°F which is similar to other chromium-alloyed steels. The toughness actually increased between 1400 (760°C) and 1500°F (815°C), which is because we are dissolving some carbide (carbides are brittle),  but not getting too much carbon in solution or grain growth. So the optimal austenitizing temperature for L6 would be around 1500°F, as that gives us a good combination of hardness and toughness. 1.2519 had flat toughness between 1400 and 1500°F though hardness also increased significantly over that range. Therefore, the hardness-toughness balance peaked at 1500°F even though the toughness did not change between 1400 and 1500°F. Toughness dropped slightly at 1550-1600°F (845-870°C), which is either due to grain growth or perhaps too much carbon in solution (I will explain that next).

With 15N20, the toughness dropped significantly even with 1500°F. In an earlier test with 15N20 I also found good toughness from 1475°F (800°C). So grain growth and a drop in toughness was found even with 1500°F, the same temperature that gave the peak properties for L6! I was surprised that toughness dropped off so rapidly for 15N20 at 1500°F, which I did not think sufficiently high to cause significant problems, even in a steel with little carbide like 15N20. This may have affected the toughness results of two 15N20 combinations I tested in my prior study, one with 1.2419 and the other with CruForgeV. 1084 is also very sensitive to overheating, grain growth, and a reduction in toughness. So despite how easy it is for 1084 and 15N20 to be hardened, I recommend using a furnace to avoid grain growth and a toughness drop.

80CrV2 and 15N20

So 15N20 needs to be austenitized at 1475°F (800°C) or below to avoid poor toughness, but 80CrV2 is more optimal from 1500-1525°F (815-830°C). Perhaps L6 is the more optimal steel to combine with 80CrV2, and 15N20 is more optimal to be used with 1084. However, the 80CrV2 can be processed to be more compatible with the 15N20. If starting from a normalized microstructure, the steel can be austenitized from a lower temperature to match the 15N20. Normalized steel is somewhat harder, and therefore more difficult to drill and bandsaw cut. With normalized 80CrV2 I found it to be about 25 Rc. This value can vary some based on the cooling rate (greatly affected by the size of the piece). If another grain refining step was added by heating to 1400°F (760°C) and air cooling, the hardness is dropped to about 19 Rc without significantly affecting the hardening response. Generally I prefer to use a “Fast DET” anneal before austenitizing instead, but this is one of the exceptions to that general recommendation.

Toughness – Carbon in Solution and Plate Martensite

Grain growth is not the only source of reduced toughness with higher austenitizing temperatures. The higher you austenitize, the more carbide is dissolved, putting more carbon “in solution,” which is why hardness is increased with temperature. However, as carbon in solution increases past 0.6% you get more “plate martensite” which is brittle and reduces toughness. You can read more about plate martensite in this article. With a steel like 15N20, the carbon content is only 0.75%, so this is not as much of an issue. However, when steels have over 0.85% carbon, they are more in danger of low toughness from plate martensite. Below is the example of O1 steel, austenitized from 1425 (775°C), 1475 (800°C), and 1550°F (845°C). Despite 1475°F not being hot enough for grain growth in O1, there was a significant reduction in toughness by austenitizing at 1475 instead of 1425°F. This was further reduced by austenitizing at 1550°F. So this is yet another reason to pay attention to optimal austenitizing ranges for different steels before combining them in pattern-welded Damascus.

Normalizing and Annealing

I know it seems slightly out of order to talk normalizing and annealing after austenitizing (to quench), but we are typically austenitizing the steel to perform these two steps as well. Compensating for normalizing is not too difficult with various Damascus combinations. It is generally best to take the higher required normalizing temperature of the two. For example, if you had combined 26C3, which needs something like 1700°F (925°C) to normalize, and combined it with 15N20 which only needs 1550°F (845°C) or so, you would normalize at 1700°F. The temperature needs to be sufficiently high to dissolve all the carbides, and the 1550°F for 15N20 would not be sufficiently high for the 26C3.

For annealing, similar rules apply. You generally want to use the higher required annealing temperature to ensure that both are annealed. If too much carbide is dissolved in one of the steels, that can mean you get pearlite at the end instead of spheroidized carbide and thus a little higher annealed hardness. But that is usually an acceptable tradeoff. As I mentioned in the 80CrV2/15N20 section, for some combinations a pearlitic, normalized structure may make the steels more compatible in heat treatment. In this case you would normalize like normal at the required temperature for 80CrV2 (1550-1650°F). Then heat to the annealing temperature for 80CrV2 (1400°F), but instead of slow cooling do air cooling. This is a grain refinement cycle instead of annealing. Normally grain refinement cycles aren’t necessary when annealing because the low temperature anneal also refines the grain. Generally I prefer annealed steel outside of specific cases such as mixing chromium and non-chromium steels. Or steel that will be heat treated in an uncontrolled forge.

I have a separate article on normalizing and annealing with recommended procedures and temperatures.

Quenching and Hardenability

Steels also have different levels of “hardenability,” or how fast they need to be quenched to be fully hardened. For example, there are “water hardening,” “oil hardening,” and “air hardening” steels. Even within low alloy non-stainless steels there can be significant differences. For example, L6 is a high hardenability oil hardening steel, while W2 is a very low hardenability water hardening steel. The two can be used together, but there is a significant gap between the two steels for hardenability. This means that to fully harden the W2/L6 Damascus you need to quench very rapidly for the W2 to ensure it fully hardens. If a slow oil was used you would likely end up with hardened L6 but soft W2. Even 1084 and 15N20 have a difference in hardenability because the 2% Ni addition in the 15N20 means its hardenability is higher despite the lower Mn. I have a loose ranking of hardenability of different steels in this article.

Tempering

Tempering leads to darker etching than untempered steel [1]. Some people using Damascus for decorative purposes (thus not needing high hardness) will skip the heat treatment but this leads to poorer contrast. Martensite etches better than ferrite, and tempered martensite etches even better.

In terms of compatibility, tempering is usually not a big deal. Most steels can be tempered at ~400°F and achieve good properties. Some steels have a slightly different range than others. 15N20 and 8670 needed to be tempered at least at 350°F for achieving high toughness and 5160 needed 375°F. The steels were not necessarily brittle below those temperatures, but did not have the high toughness the steels are known for.

You can also see that the toughness of 15N20 dropped when tempering at 450°F, which is called “Tempered Martensite Embrittlement.” The temperature at which TME is first seen changes some by steel, and some do not see the phenomena until 500°F or even higher. However, 400°F is safe for any steel I have so far tested.

Toughness and Edge Retention

I already have a whole article on the testing of toughness and edge retention of pattern-welded Damascus so I won’t rehash all of that here. But there are a few key points to mention here when it comes to compatibility:

  1. Combining a low toughness and high toughness steel generally seems to lead to toughness similar to the low toughness steel. It fractures at the “weakest link” and there isn’t much benefit to adding a high toughness steel in terms of overall toughness.
  2. High wear resistance steels with high slicing edge retention generally still cut very well even when combined with a steel with lower wear resistance. So combining CruForgeV and 15N20 or ApexUltra and L6 led to edge retention similar to CruForgeV or ApexUltra. However, this was due in part to the improvement in edge retention seen in ladder patterning.
  3. While ladder patterning benefited edge retention it also slightly reduced toughness.
  4. A “Damascus Cutting Effect” was seen in a 1095/Nickel Damascus. Most steel combinations do not have hard and soft layers but using nickel does provide this potential benefit.

When not attempting to have the “Damascus Cutting Effect” it can be beneficial to have two steels with good wear resistance. For low alloy non-stainless steels it makes sense to look at steels with significant vanadium and/or tungsten additions like ApexUltra, CruForgeV, 1.2519, 1.2419, 1.2562, Blue Super, V-Toku1, etc. However, for low alloy steels the main choices for a “bright” layer are 15N20 and L6 and neither has much wear resistance.

If making a Damascus combination for high toughness there must be two high toughness steels. 1084 and 15N20 are a decent combination for this. 1084 is somewhat lower in toughness but the two together still tested at ~34 ft-lbs in a random pattern (as opposed to 45-50 ft-lbs for 15N20).

Summary and Conclusions

It is best to choose steels that have similar temperatures for heat treating. High manganese is best for a dark layer after etching while Nickel is best for a bright layer. Other alloying elements can make forge welding difficult when using conventional flux methods, especially high levels of chromium. It is important to adjust heat treatment based on the steels that are combined together. For example, 15N20 sees a large toughness drop when austenitized at 1500°F. So when 1084 and 15N20 are used together it is best to heat treat with a furnace so that the steel isn’t overheated. The optimal temperature range for austenitizing 80CrV2 is too high for 15N20. If 80CrV2 and 15N20 are used together it is better to use a normalized starting structure so that a lower austenitizing temperature of 1475°F (800°C) can be used with the 80CrV2 and still achieve high hardness. L6 may be more optimal than 15N20 to use along with other chromium-alloyed steels though it has lower nickel than 15N20 (thus contrast is not as good), and is also more difficult to work with because of its alloy additions. High carbon steels are more sensitive to overheating because the grain boundaries melt, leading to crumbling during forging. High vanadium and tungsten steels are best for high wear resistance combinations, though they typically need to be combined with 15N20 or L6 which unfortunately do not have much wear resistance.


[1] Verhoeven, John D., and Howard F. Clark. “Carbon diffusion between the layers in modern pattern-welded Damascus blades.” Materials characterization 41, no. 5 (1998): 183-191.

[2] Meilach, Dona Z., George Martin, E. A. Chase, and Theodore Davidson. “Decorative and sculptural ironwork: tools, techniques, inspiration.” 1977.

[3] Dunkerley, Rick. “His Forge Burns Hot for Mosaic Damascus.” Kertzman, Joe, ed. Blade’s Guide to Making Knives. Krause Publications, 2005.

[4] https://www.kovares.com/product-page/165mm-damascus-petty

The post Is 1084-15N20 The Best? Pattern-Welded Damascus appeared first on Knife Steel Nerds.

  •  

Coatings vs Foil – Heat Treating Steel

Thank You Patreon

Thanks to my Patreon supporters I was able to buy all of the coatings to test for this article. If you want to support more knife steel research come join us at Patreon.com/KnifeSteelNerds

We have a great community, you get to see articles and videos before everyone else, and at the top tier you even get a free Knife Steel Nerds mug.

YouTube Video

I have a video version of the following information:

Why Protect the Surface?

There are two things we are trying to prevent by protecting the surface during heat treating: scale and decarburization. I frequently see knifemakers confusing these two things. Scale is not decarburization, and removing scale does not mean that the layer of decarburization is removed. Scale is the black iron oxide that forms on steel at high temperature in the presence of oxygen. During forging of steel it is common to see this scale come off in flakes.

A bar of 4340 steel with black scale on it

However, the oxygen doesn’t only interact with the iron, but also carbon. The carbon leaves the steel at the surface after forming carbon dioxide or carbon monoxide. This leads to a layer of steel with very low carbon, called a “decarburization layer.”

Problems from Decarburization

This decarb layer doesn’t harden because of the lack of carbon. However, unlike scale, a decarburization layer is still steel so it can be difficult to see without etching in acid first. So sometimes knifemakers are measuring low hardness or easily scratching with a file because they are unaware of this decarburization layer. That soft layer will also obviously affect performance, if an edge is sharpened within the “decarb” layer it will be soft and the knife won’t hold an edge. It can also affect aesthetics because the soft steel will polish differently. Another common issue can be warping and distortion from the decarb layer. This layer being free from carbon means that it will transform to other phases at a different temperature than the rest of the steel. The uneven transformation leads to different size changes within the steel leading to warping.

Protective Atmosphere and Salt Pots

If no oxygen is present, scale will not form and decarburization will not occur. So if the steel is heat treated in a vacuum furnace or within a protective atmosphere like argon then scale and decarb are not issues. With salt pots the steel is within molten salt without an atmosphere, so again there is no scale or decarb. However, these solutions are not always practical so other ways of protecting steel are often used by individual knifemakers with simple heat treating equipment.

Foil

A common method for preventing scale and decarb is to use a heat treating foil. The steel is wrapped in the foil and then each exposed side is folded over at least twice to prevent air from entering the packet. The foil is thin and on the outside so it heats up first and oxidizes which further eliminates oxygen left within the packet.

There are two major types of heat treating foil: 321 and 309 stainless steels. The 321 foil is rated up to 2000°F and the 309 is rated up to 2240°F. The 309 is more expensive than 321. The 321 stainless also has a small titanium addition which is also claimed to help with reacting with oxygen inside the packet [1]. Foil is very sharp so gloves should be worn when handling it. Some people recommend adding paper or oil to burn up inside the packet but this is not necessary. Some people recommend talcum powder to prevent sticking though I haven’t tried it. Reusing foil is not recommended because the foil has already oxidized and also becomes brittle.

The main limitation of foil is for oil or water hardening steels because removing the foil prior to quenching is very difficult within a reasonable time. With air hardening steels the foil works well with a “plate quench” because when the plates are held tight the heat will steel conduct through the foil.

Coatings

Various coatings are also available that are designed to protect steel from scale and decarb during heat treating. These are especially useful for oil and water hardening steels since no foil needs to be removed. I used several different coatings for my recent experiments:

ATP-641 [2] – a water based ceramic coating that is rated up to 2300°F. It can be sprayed, dipped, or brushed.

NoScale2000 [3] – another water based coating that is rated up to 2000°F. The coating is made by Daniel O’Connor for knives. It can be sprayed or brushed. O’Connor also makes a version made for developing a hamon called Hamon1800.

Turco Pretreat [4] – This product is also named Bonderite L-FM Pretreat Aero. It is a paint, so the texture is quite different than the two above. The primary recommendation is to spray this coating though I used it by dipping. The datasheet does not list a maximum temperature.

Condursal Z1100 [5] – Another paint coating like Turco. Rated up to 1100°C (2012°F). Can by applied by brushing, dipping, or spraying.

Experiments

I did three experiments with the different coatings. Each used a 1/8 x 3/4 x 1-1/2 inch (19 x 38 mm) coupon. They were finished to 120 grit and cleaned with soap and water prior to dipping in one of the coatings, followed by letting them dry for 24 hours. The 1095 coupons were only finished to 60 grit and the Condursal Z1100 coupons were only finished to 60 grit. I also tried brushing the NoScale2000 which I will explain in that section. A “bare” sample was also tested with each without a coating.

1. 1095 steel heated to 1475°F for 10 minutes, quenched in Parks 50 oil. This is to test the effect of each coating on the quench since 1095 is a water hardening steel and needs a fast quench.

2. 52100 steel heated to 1550°F for thirty minutes, quenched in Parks 50 oil. This is a relatively standard datasheet heat treatment for 52100. It is on the high end for temperature and time for oil/water hardening steels so it serves as a good test of how much decarb happens for these types of steels.

3. AEB-L steel heated to 1975°F for 30 minutes, then quenched in Parks 50, then placed in liquid nitrogen for an hour. For the AEB-L I also added a sample that was  wrapped in foil prior to a plate quench and then liquid nitrogen. This was a test to see how the coatings did near their temperature limit. Also to see how much decarb happens at this relatively high temperature.

For each coupon I took pictures after cleaning them to see the amount of scale from each. I did microscopy of the cross-section for ATP-641, NoScale2000, and Turco but I didn’t get the Condursal until later so no microscopy for that coating. I also measured hardness for all of them.

Uncoated Coupons

The 1095 coupon formed only a small amount of scale because it was heated to a relatively low temperature of 1475°F (800°C) for a short time of 10 minutes.

1095 coupon heat treated without a coating

The 52100 coupon heat treated at 1550°F for 30 minutes had significantly more scale and it was very dark in color. Some came off when cleaning the oil off the coupon.

52100 coupon heat treated without a coating

The AEB-L coupon heat treated at 1975°F for 30 minutes was not as dark as the 52100 coupon and the scale was a bit less even.

AEB-L coupon heat treated without a coating

Looking at the cross section, the 52100 has a thin decarb layer and thin layer of scale. The AEB-L, however, had a very thick decarb layer measuring over 0.2 mm (~0.01 inches).

52100 uncoated coupon cross section

AEB-L uncoated coupon cross section

1095 Quenching Experiment

I decided to do the quenching experiment based on an earlier experience. A knifemaker contacted me about difficulty with heat treating 80CrV2; it wasn’t hardening. We talked through the process and he told me he was coating each blade with ATP-641. I recommended he try it without the coating and he didn’t have any problems after that.

All of the 1095 specimens fully hardened to 66-67 Rc and this was true at the surface as well as after grinding 1 mm into the specimen. The one exception was the NoScale2000, which was about 36 Rc. I repeated the experiment to make sure it wasn’t a fluke and got 33 Rc. In both cases the coating did not come off during quenching and I had to clean it off to be able to test hardness. I saw that O’Connell recommended brushing on the NoScale2000 rather than dipping so I tried it again by brushing it on. In this case the steel fully hardened.

1095 NoScale2000 coupon after quenching in Parks 50 oil. The coating remained on the steel.

I did not find an issue with hardening the 1095 with ATP-641 despite the prior issue the knifemaker experienced with 80CrV2. However, I do think that there is significant “danger” to quenching slowly with coatings applied. Ensuring the coating is not too thick helps with quenching as expected.

NoScale2000

Another puzzling thing was that the NoScale2000 appeared to lead to even more scale than when heat treating it without any coating. The repeat experiment of 1095 also led to a lot of scale. When I brushed on the NoScale2000 there was still scale that formed it was just more “spotty.”

1095 “bare” coupon (heat treated without a coating)

1095 NoScale2000 dipped coupon #1

1095 NoScale2000 dipped coupon #2

1095 NoScale2000 brushed coupon

The 52100 coupon coated with NoScale200 also had a somewhat spotty appearance similar to the 1095 brushed coupon. The AEB-L NoScale2000 coupon looked at least as bad as the uncoated coupon, perhaps worse.

52100 NoScale2000 coupon

AEB-L NoScale2000 coupon

Looking at the cross-sections, the 52100 coupon looks very similar to the uncoated coupon. The AEB-L coupon has a decarb layer of approximately the same thickness as the uncoated coupon.

52100 NoScale2000 cross-section

AEB-L NoScale2000 cross-section

I let Daniel O’Connor know about my subpar results and he said that, “[Y]our results are not typical of my user base.” He told me about good experiences many knifemakers have had using it. If you have had better experiences with the NoScale2000 let us know in the comments.

ATP-641 Coupons

Surprisingly the 1095 coupon coated with ATP-641 had some spotty scale that formed, not looking too different than the uncoated coupon. The 52100 coupon, however, didn’t have any obvious scale just some discoloration. But the AEB-L coupon formed scale and didn’t look very different than the corresponding uncoated coupon.

1095 ATP-641 coupon

52100 ATP-641 coupon

AEB-L ATP-641 coupon

Looking at the cross-sections with metallography there is no obvious decarburization in either the 52100 or the AEB-L. This is somewhat surprising given the rough scale that formed on the AEB-L. Maybe the ATP-641 affected the surface in some way on its own while still preventing decarb.

52100 ATP-641 cross-section

AEB-L ATP-641 cross-section

Turco Coupons

The 1095 Turco coupon had some scale that formed, lining up with the grinding marks. Perhaps this was because of the coarser 60 grit finish on the 1095 coupon vs the 120 grit on the 52100 and AEB-L coupons. The 52100 coupon had some discoloration and it is hard to tell if it was scale or not but otherwise looked good. The AEB-L perhaps had some light scale that formed but otherwise looked very good.

1095 Turco coupon

52100 Turco coupon

AEB-L Turco coupon

There was no apparent decarburization visible in the metallography analysis of the 52100 coupon. The AEB-L coupon also looked good apart from one corner where presumably the Turco had rubbed off prior to heat treatment.

52100 Turco cross-section

AEB-L Turco cross-section

Condursal Z1100 Coupons

The Condursal seemed to be very similar to the Turco apart from color (green vs orange paint). The resulting coupons also looked pretty similar to the Turco coupons. For some reason there was more scale on the 52100 coupon. And the rougher 60 grit finish I did with these followup coupons also seemed to affect the amount of scale that formed somewhat. I did not do metallography with these coupons.

1095 Condursal Z1100 coupon

52100 Condursal Z1100 coupon

AEB-L Condursal Z1100 coupon

Foil

I only used foil with AEB-L. As expected the steel came out completely clean apart from some rainbow coloration from the small amount of oxygen left in the packet.

AEB-L foil coupon

Surprisingly there is what looks like a thin decarb layer visible in the cross-section. Perhaps the little bit of oxygen that interacts with the steel is enough for a small amount of decarburization.

AEB-L foil coupon cross-section

User Error?

This is my first time using many of these coatings so there can certainly be criticism of my technique. Dipping into the coating did not seem like the very best way to apply most of them. The one I thought had the best texture for dipping was the NoScale2000 which was also the one that didn’t come off when quenching. The Turco and Condursal recommend very thin coatings in the datasheets but I was concerned some of it might have been running off while drying. The coating thickness did not appear to be even. Perhaps spraying would have been better for some/all of these coatings. I attempted brushing the coatings on but didn’t like it; even letting them dry in between coats seemed to lead to me brushing off as much as I was brushing on. The surface finish also appears to matter with these coatings, a finer finish is better. And they need to be clean of course.

Scale-X

One coating I found about too late is Thermodur Scale-X. It is a paint-based coating that comes in a spray can so you don’t need a dedicated sprayer. Based on my experience with the coatings in this article I think spraying might be better so this sounds very convenient. And the two paint-based coatings I tried worked well. So I will be getting some to test it.

Summary and Conclusions

Coatings can be useful in certain instances for oil and water hardening steels. I had somewhat inconsistent results with them. I also found that the amount of decarb is relatively small at temperatures typical of water and oil hardening steels (less than 1600°F/870°C) so it depends on how much of a hassle you think applying the coatings is. If you plan to remove material through grinding after the coatings may not be necessary for low alloy steels. Thoroughly cleaning the steel and having a fine finish is helpful for the coatings to work at their potential. Learning to effectively apply them likely requires some trial and error. I wasn’t totally happy with dipping or brushing them on, may spraying is better. For steels that require high temperature, in this case AEB-L, I was able to prevent decarb with the coatings except for NoScale2000. Decarburization is quite significant without any type of protection and should definitely be avoided. The Turco and Condursal coatings led to a more scale-free surface than the ATP-641 and NoScale2000. I greatly prefer foil for heat treating air hardening steels.


[1] https://www.toolwrap.com/pages/all-about-tool-wrap?srsltid=AfmBOoqG9o8GgfgNq8u2WT2Eh9IeyYGLYITqxhqOkq-qoc1ENjuQ2joR

[2] https://atp-europe.com/wp-content/uploads/2023/08/ATP-641.pdf

[3] https://nuclayer.twinoaksforge.com/product/noscale-2000-16oz/

[4] https://webaps.ellsworth.com/edl/Actions/GetLibraryFile.aspx?document=12319&language=en

[5] https://www.theduffycompany.com/condursal-z1100/

 

The post Coatings vs Foil – Heat Treating Steel appeared first on Knife Steel Nerds.

  •  

How to Anneal Stainless Steel After Forging

Another rather large heat treating study! This one took quite a bit of time, effort, and money. If you want to support further research visit Patreon.com/KnifeSteelNerds and become a Patreon supporter. All of the money I receive that way goes to knife steel research. And you get some perks like seeing articles and videos early, and at a high enough tier you get a free Knife Steel Nerds mug!

Video 

Here is the video version of the following information:

Should Stainless Steel Be Forged?

Stainless steels are generally more difficult to move under the hammer than simple carbon and low alloy steels. They are typically more expensive. The forging range is usually narrower; you have to stop forging at a higher temperature or it may fracture. But of course stainless steel has the major advantage that it is corrosion resistant. There are many myths around forging stainless and carbon steels that are used to justify the use of only simple steels. These myths scare some knifemakers away from using stainless steels that might otherwise try them.

Is Stainless Steel Improved by Forging?

There is an old tradition in the knife world that says that only carbon steels should be forged. Some have gone so far to say that stainless steels do not “benefit” from forging in the same way that carbon steels do. This is somewhat difficult to refute, as the benefits of forging are often overblown to begin with. I have an older article on forging vs stock removal you can read here. However, I argue that high alloy tool steels and stainless steels have more potential benefits to forging than low alloy steels. The reason is because with simple steels all of the carbides are dissolved at forging temperatures and re-precipitated later; this makes the carbide structure easier to control with thermal cycling alone. High alloy steels have carbides that do not dissolve without melting the steel itself so there is more possibility of improving that structure through further working. Of course all steel purchased by knifemakers has already been forged and/or rolled from an ingot, so we are often talking about a relatively small amount of further forging.

D3 tool steel forged to different degrees thickness starting from a 10″ round ingot [1]

And the carbide structure has directionality to it, leading to different properties in the longitudinal and transverse directions (along the rolling direction and perpendicular to it). In my forged vs stock removal article I gave reasons for why forging blades to shape rarely leads to superior toughness, but if such a benefit was to be gained it would be more pronounced in high alloy and stainless steels.

M7 high speed steel with different degrees of reduction [2]. You can see that the carbide bands are elongated along the rolling direction.

What is a High Alloy Tool Steel?

Most of the information in this article will relate to not only stainless steels but also high alloy tool steels like A2, D2, CPM 3V, etc. Stainless steels used in knives are simply a subcategory of high alloy tool steels. Low alloy tool steels and simple carbon steels behave somewhat differently like 1095, O1, 52100, 80CrV2, and others. The line between low and high alloy can be somewhat fuzzy, some give it as 5% total alloy content. So if the chromium, tungsten, molybdenum, etc. add up to more than 5% it is high alloy. For our purposes a high alloy tool steel is any with at least 3% chromium. These steels are air hardening and their carbides dissolve at higher temperatures. This does not mean all of these steels will be annealed with exactly the same temperatures, hold times, cooling rates, etc. but similar ideas will apply to them.

How Hot to Forge Stainless and High Alloy Tool Steel

A common mistake with forging of stainless and high alloy tool steels is heating the steel too hot. It is a common misconception that because the steel is more difficult to move under the hammer that more temperature is necessary. When steel is overheated, the grain boundaries melt first, leading to steel breaking apart when it is forged. Some knifemakers mistakenly assume they must not have been hot enough, and try even hotter! The temperature at which grain boundaries melt is roughly the same with stainless steel as it is with simple carbon steels, and sometimes lower. Datasheets typically recommend 2100°F (1150°C), though some will recommend lower like 1900-2000°F (1035-1100°C). 2100°F/1150°C seems to work for most knifemakers I speak to. However, many knifemakers are used to lower carbon steels like 1084 or 80CrV2 which can handle higher temperatures and they are not used to dialing the forge down for higher carbon steels. This is why “cast iron” has very high carbon content (>2%); higher carbon means lower melting temperature so it is easier to melt the cast iron before casting. High carbon steels that are more commonly used in forging like 26C3, White #1, Blue Super, and ApexUltra are also more sensitive to overheating since they have relatively high carbon contents (>1.2%).

How to Normalize Stainless Steel

Stainless and high alloy steels are not normalized. The goal of normalization is not grain refinement but rather dissolving all of the carbides before air cooling. As I noted above, with most stainless steels the carbides do not dissolve until melting. Perhaps we could come up with some kind of creative treatment that could improve/change the microstructure prior to annealing but this is not common in the steel industry. Normalizing is not necessary and we will be skipping it with stainless and high alloy tool steels.

What Are We Trying to Accomplish During Annealing?

Annealing is the step we perform between forging and the final austenitize and quench. The steel is annealed by the manufacturer before you get it. For stock removal makers, annealing is not necessary except in rare circumstances. The purposes of annealing are multi-fold:

  1. Soften the steel so it is ready for machining, drilling, bandsaw cutting, etc.
  2. Prepare the steel for good response to austenitizing so that we don’t need excessive hold time or temperature.
  3. Maximize the final properties after heat treatment including hardness, toughness, etc.

Problems with Annealing Stainless Steel – Long Times, Scale, and Decarburization

One issue with annealing stainless steel is that the recommended annealing procedures often require cooling from 1600F+ down to 1000F at 25 degrees Fahrenheit per hour (~15°C/hr). That takes over 24 hours! Not only does this take a long time but most knifemakers do not have furnaces equipped with inert gas or vacuum so this means that scale and decarburization are major concerns. Without any protection you could end up removing a significant amount of carbon from the steel. To mitigate this it is best to wrap the steel in foil during annealing. I found double wrapping to help some as well. This is not a surefire way to prevent any scale or decarb as the times are very long. Therefore it is best to leave some material to remove after heat treating to ensure all of the scale and decarb is removed. I have not experimented with coatings for annealing but they may also work.

Why AEB-L is a Good Stainless to Start With

The first steel I experimented with was AEB-L. It checks a lot of boxes for forging bladesmiths as it is a very fine carbide steel with properties that can be similar to low alloy and simple carbon steels. Some have called it “stainless 52100” for its fine carbide size and excellent toughness. It is also relatively low cost, as some bladesmiths have sticker shock buying expensive stainless steels when they are used to buying 1084 or 80CrV2 for less than $5 per pound. AEB-L’s relatively low carbide content also means it is somewhat easier to forge than other stainless steels; I have an article on which steels are most difficult to forge here. Having only chromium carbides means it is easier to grind and finish than some of the more exotic stainless and high alloy tool steels with very hard vanadium carbides. One potential downside to AEB-L is it is not typically available thicker than about 1/4″ (6 mm), so bladesmiths that like to forge from heavy stock, round bar, etc. will be out of luck.

My New Experiment with AEB-L

We started with 1/4″ AEB-L which my father, Devin Thomas, hot rolled down to 0.130″ (3.3 mm), which is a bit less than a 50% reduction. The temperature used for rolling was around 2100°F. I then annealed it in different ways and measured the annealed hardness, hardness after quench and temper, and toughness after quench and temper. The different annealing procedures I tried will be given in the sections below. The final austenitize I used was 1925°F (1050°C) for 15 minutes, plate quench, cryo in liquid nitrogen, then double temper at 350°F (175°C).

Traditional Slow Cool Annealing

I have an earlier article that discusses the mechanisms within steel that occur during annealing. The typical method is for heating the steel to a temperature where the steel is austenitic (the high temperature, nonmagnetic phase of steel), but typically lower than austenitizing before quenching. For a simple carbon or low alloy steel this is somewhere in the range of 1350-1450°F (730-790°C) while austenitizing before quenching is typically 1475-1550°F (800-845°C). This lower temperature means more carbide is present, then during slow cooling the soft ferrite forms while feeding carbon to those carbides and growing them, resulting in a “spheroidized” structure (round carbides).

Carbides increasing in size during slow cooling as the ferrite grows into the austenite

There are a couple differences with high alloy and stainless steels. For one, the temperatures for annealing are typically higher, with 1600-1650°F (870-900°C) being most typical. The steels do not transform to austenite until higher temperatures, necessitating the higher temperatures. Typically the hold time is longer at this temperature as well, such as two hours. Following that hold time, the cooling rates are also slower. These are “air hardening” steels so they are more prone to hardening if the cooling rates are not sufficiently slow. This is partially why low cooling rates like 25°F/hr are recommend in datasheets, though that is also true in many datasheets for low alloy steels. So for AEB-L I wanted to try 50°F/hr and 100°F/hr and see how the resulting properties compared with the as-received steel from the manufacturer. The temperature you must cool to for ensuring full transformation depends on the cooling rate and the steel. However, most annealing procedures will recommend a temperature below which no more transformation is likely to occur, such as 1000°F. I used 1100°F for the 50°F/hr anneal and 1000°F for the 100°F/hr anneal. If the steel is fully transformed it doesn’t particularly matter what cooling rate is used below that temperature.

The hardness after annealing was at first a bit surprising because even with the fast 100°F/hr the hardness was significantly lower than what is delivered by Uddeholm (As-received). Perhaps Uddeholm uses an even more rapid form of annealing.

AEB-L As-Received by Uddeholm

50°F/hr anneal

100°F/hr anneal

This hardness difference appears to be confirmed by the metallogaphy, as the carbides in the two anneals I performed have somewhat larger carbides. I next compared the resulting hardness and toughness with prior toughness testing done with the as-received steel.

The same 1925-350 heat treatment with the as-received material (labeled “Stock Removal”) is the 60 Rc point. So the 50°F/hr anneal resulted in slightly lower hardness with equivalent toughness, and the 100°F/hr anneal resulted in slightly better hardness and toughness. This is mildly surprising based on the annealed hardness and somewhat larger carbides in the annealed condition. But overall this is a good result, with the 100°F/hr anneal being relatively fast, having very low annealed hardness for ease in working, and then excellent hardness-toughness after final heat treatment.

Isothermal Hold Annealing

Another similar way to anneal is to do a hold at a lower temperature rather than a slow cool. After heating to 1600°F like with the prior annealing, I held at either 1300°F (700°C) or 1200°F (650°C). Holding at a higher temperature is roughly equivalent to a slow cooling rate, while holding at a lower temperature is equivalent to a faster cooling rate. I held at 1300°F for 4 hours and 1200°F for 6 hours, as I was concerned it would take longer at the lower temperature (based on published transformation curves for stainless steels).

I also decided to try a technique that is common with low alloy steels which is to do “grain refining” cycles prior to the 1300°F anneal. I heated to 1600°F for 30 minutes and air cooled, which I did twice before the same anneal. I did not find grain refining cycles to improve properties in 1084 in a prior experiment, but I thought it wouldn’t hurt to try it again. I labeled this condition “cycled.”

These were somewhat closer in hardness to the as-received condition. However, oddly the hardness of the 1200°F condition  was lower than the 1300°F. Yes I held it longer at that temperature but the transformation was completed in both cases (as will be shown in the metallography), so that should not have been a factor.

Isothermal Anneal 1300°F

1200°F Isothermal Anneal

The 1200°F anneal looks like it resulted in somewhat finer carbides thought they don’t look that different. And both look relatively similar to our slow cool anneals. There are probably subtle differences if we did a full statistical analysis, but the real differences are probably more apparent through the annealed hardness and the final heat treated hardness and toughness.

The properties look pretty similar between the three and I’m not sure there are any “real” differences between the three. They are all around 60.5 Rc and ~35 ft-lbs. Maybe the grain refining cycles or the lower 1200°F led to a slight improvement but those small improvements may disappear if we did the experiment multiple times and averaged the results.

Temper Annealing

Another type of annealing is quite different than the others which is temper annealing, which I have written about before. In fact this is the general type of annealing that I recommended for high alloy steels in Knife Engineering. With normal tempering of martensitic steel, the higher you temper the softer the steel gets. If you temper hot enough you get annealed, soft steel. However, normally we do an austenitizing and quench step from a lower than normal temperature prior to a very hot temper. I recommended this annealing treatment because of older studies that showed a superior grain size and toughness with high speed steels after a temper anneal rather than a more conventional anneal. But the tempering times for optimal properties were very long, 12-24 hours depending on steel and tempering temperature. Also I began to be worried that perhaps the anneal was better only for high speed steels, since they use very high austenitizing temperatures where grain growth is more common. Perhaps the temper anneal resulted in more stable carbides that don’t dissolve as readily at the high temps, therefore they still pinned the grain boundaries. For most steels where grain size is not as difficult to control, this benefit would be lost.

So based on those prior reported experiments I austenitized all of them at 1600°F for two hours prior to plate quenching. This also has the benefit of maintaining the same austenitize as the prior annealing experiments. I then tried three different tempering conditions: 1300°F 4 hours (Q13), 1400°F 4 hours (Q14), and 1400°F 24 hours (Q24). Long anneals were optimal for the high speed steels but I wanted to have shorter anneals which is why I also tried the 4 hour tempers.

The 1300°F anneal (Q13) is definitely harder than we would desire. The 1400°F for 4 hours (Q14) is better, and the 24 hour anneal (Q24) is definitely soft enough. Maybe we could do something in between 4 and 24 hours with 1400°F instead.

Q13 – 1300°F 4 hour temper anneal

Q14 – 1400°F 4 hour temper anneal

Q24 – 1400°F 24 hour temper anneal

Only the Q24 looks properly annealed with medium size spheroidized carbides throughout. The Q13 condition specifically has relatively large regions which still look like martensite, or only very small spheroidized carbides.

Comparing the toughness, Q24 and Q14 are very similar, while the Q13 was significantly worse. The average hardness I measured with the Q24 was around 60 but I got several readings that were lower; overall it seemed to test less consistently. Maybe that means the carbides were too coarse, again pointing to an optimal hold time being somewhere between the 4 and 24 hours I tested with 1400°F. The Q13 ended up being slightly lower in hardness which is just randomness. I did another set of small hardness coupons and it was more similar to the Q14. My hypothesis for why the Q13 had worse toughness is related to the inconsistent microstructure. Maybe those martensite regions led to large grains because there weren’t carbides available to pin the grain boundaries.

AEB-L Annealing Summarized

When looking at all of the conditions as a whole, the overall finding was that if we have properly annealed the steel the properties are relatively similar. We got good (low) annealed hardness with most of them, and the resulting hardness and toughness were also pretty similar. My favorite of the conditions was the 100°F/hr anneal. The overall time to anneal is around 8 hours, meaning you can anneal it overnight after forging the steel. And it had the best combination of hardness and toughness after the final heat treatment of 1925°F austenitize and 350°F temper.

Annealing MagnaCut

I also wanted to look at a steel that may require a slower cooling rate than AEB-L so I also tested MagnaCut. Of course I developed MagnaCut so I was more interested in it. But the reason why MagnaCut was a good steel to look at is because of its 2% Mo. Molybdenum increases “hardenability” of steel so that larger sizes can be air cooled and still fully harden. This also affects annealing. Below I have Time-Temperature-Transformation (TTT) curves for two steels after they were austenitized at a low temperature for annealing:

D2 Annealing TTT after austenitizing at 1600°F

M2 annealing TTT after austenitizing at 1625°F

It can take a minute to understand the charts if you have never looked at them before. The curve to the left shows how long it took for the steel to start transforming, and the curve to the right shows how long it took for the transformation to end. For D2 with 0.74% Mo, at the fastest transformation temperature (~1400°F) it took less than 30 minutes to fully transform. For M2 with 5% Mo (and 6.5% W), it took over 3 hours to fully transform at the same temperature. This is largely cause by the Mo difference. So I was concerned that a 100°F/hr anneal may not work with a steel like MagnaCut with 2% Mo. This should then translate to the many stainless steels with less than 2% Mo (440C, Elmax, M390, S90V, etc.), and to the several stainless steels that also have around 2% Mo (S30V, S35VN, S45VN, S110V). The most common steel with even more Mo is 154CM/CPM-154 with 4% Mo though its datasheet says it can fully transform at 1300°F after 4 hours so there is a decent chance it can also use an intermediate cooling rate.

We did the same experiment of hot rolling MagnaCut from 1/4″ down to 0.130″, I performed a few different annealing cycles from 50°F/hr or 100°F/hr and measured the annealed hardness. However, I also wanted to experiment with the annealing temperature prior to cooling so we looked at that for this steel. We will get to that after we take a small detour to discuss how those annealing temperatures are chosen.

How to Select an Annealing Temperature

Most steels have an available datasheet that lists a recommended annealing procedure. For example, the MagnaCut datasheet recommends the following for annealing: Heat to 1650°F (900°C), hold 2 hours, slow cool no faster than 25°F (15°C) per hour to 1100°F (595°C), then furnace cool or cool in still air to room temperature. So if you follow my recommendation and use the faster cooling rate of 100°F/hr you can simply use that recommended temperature (1650°F/900°C), and then cool at the faster rate.

But what if the steel does not have a datasheet, or the datasheet doesn’t give an annealing temperature? At that point we need to find the temperature at which the steel has transformed to austenite. With a simple carbon or low alloy steel that can be done with a magnet because austenite is non-magnetic. However, there is another point where steel becomes nonmagnetic called the “Curie point,” and high alloy steels reach that point before they transform to austenite. So another way we can try to determine it is to heat the steel to different temperatures and quench and see the point where hardness increases. I did this with both AEB-L and MagnaCut:

You can see that AEB-L shows a rapid increase in hardness between 1400 and 1475°F which is the region over which it transforms from ferrite to austenite. After it transforms to austenite, carbon goes in solution, then you can quench and the hardness is much higher after quenching. However, if you quench after heating to 1400°F, you didn’t transform to austenite and the hardness stayed low. It looks like we could anneal AEB-L from as low as around 1500°F, and the 1600°F I chose for my study should be pretty safe.

With MagnaCut, however, the transition is more difficult to see because carbon doesn’t go into solution until a higher temperature. It looks like the steel may have started transforming to austenite around 1550°F but this actually led to the steel slightly decreasing in hardness. The steel started increasing again around 1650°F and I think this means it is likely where austenite finished transforming and is probably a reasonable temperature to anneal from. But I wanted to see how the annealing temperature would affect the annealed hardness and the final heat treated properties.

There were several surprises in this experiment to me. One is that the temperature mattered much more than the cooling rate, at least for those two cooling rates. The other surprise is that the change in annealed hardness was quite linear. There was no big jump in hardness from annealing at too low of a temperature, even at 1550°F. The “as-received” hardness for annealed MagnaCut is around 22 Rc which is similar to the hardness measured for the 1600°F anneal.

The next experiment I wanted to do was ensure that we were getting good properties from annealing at 1650°F since the annealed hardness continued lower up to 1750°F annealing temperature. And the as-quenched hardness we measured from MagnaCut before didn’t really go up significantly until 1700°F. So I heat treated coupons from the 1650, 1700, and 1750°F anneals with both cooling rates. This also allowed me to compare properties with the two different cooling rates:

The hardness after heat treating was slightly higher with the faster annealing rate, which we would expect to see from having somewhat finer carbides. There wasn’t much difference between 1650 and 1700°F though there was a small drop by increasing to 1750°F. So I would probably recommend sticking with the 1650-1700°F range for annealing MagnaCut.

The toughness was slightly higher for the 50°F/hr anneal in line with its slightly lower hardness. Both the 50°F/hr and 100°F/hr anneals resulted in somewhat higher hardness than the as-received condition. You could austenitize somewhat lower or temper somewhat hotter to reduce the hardness if desired. The forged and annealed MagnaCut had a slightly higher hardness-toughness balance than the as-received material. However, toughness testing can be somewhat variable and I have managed to get ~16 ft-lbs with 62 Rc as-received before. I think the toughness may be slightly better or slightly more consistent with the forging and annealing. Probably not enough to justify forging blades instead of doing stock removal, but I have also heard some bladesmiths claim that you will “ruin” stainless steel by forging it yourself and that is certainly not the case if you do it right. I also don’t think that toughness results of forged low alloy and simple carbon steels are enough to justify forging. Knifemakers should choose forging or stock removal based on other factors.

Summary – General Stainless and High Alloy Tool Steel Recommendations

Don’t forge too hot – 2100°F is a good target temperature. A common mistake is thinking that stainless steels need higher temperatures to forge. They do not.

Don’t forge too cold. Stainless and high alloy tool steels need higher minimum forging temperatures. They become “hot short” (brittle) at higher temperatures than simple carbon steels. Depending on the steel and the datasheet, this minimum is given in the range of 1650-1750°F (900-950°C).

Protect the steel from atmosphere during annealing – Vacuum or inert gas is best but for many knifemakers this means double wrapping in foil (not double folding but double wrapping), and leave some extra steel to grind away.

Choose the right annealing temperature – Typically in the range of 1600-1650°F for most stainless and high alloy steels but can sometimes vary. Check for a datasheet if a temperature recommendation is given and that temperature should work fine. A 2 hour hold at the temperature is typical. If no datasheet temperature is available you may be able to use the method shown above with AEB-L and MagnaCut where I found the temperature at which the hardness goes up, indicating that austenite formed.

Cool at 100°F/hr – This is significantly faster than recommendations given in most datasheets but gives a better balance of speed (~8 hours instead of 24+, can anneal overnight) and final properties (higher final hardness and toughness). There may be some steels that cannot handle this faster cooling rate if they have very high Mo contents. If the steel ends up higher than 25 Rc at the end it may need slower. As a side note, 100°F/hr was also found to be optimal with ApexUltra, a low alloy steel, so maybe we are on to something here.

Cool to 1000-1100°F, after that the cooling rate can be faster. You can experiment with whether the final cooling point can be higher than 1000 or 1100°F by annealing both ways and seeing if the hardness is the same. Once the transformation is done, further cooling doesn’t matter. I probably wouldn’t go any higher than 1200°F in any case. This really only matters if that extra hour or two will significantly impact your workflow.

So to summarize, anneal at 1600-1650°F for two hours, slow cool at 100°F/hr to 1000°F. Before that don’t forge too hot or too cold, and protect it from atmosphere during annealing.


[1] Roberts, G A, and Robert A. Cary. Tool Steels. Beachwood, Ohio: American Society for Metals, 1980.

[2] Roberts, George Adam, Richard Kennedy, and George Krauss. Tool steels. ASM international, 1998.

The post How to Anneal Stainless Steel After Forging appeared first on Knife Steel Nerds.

  •  

AR-RPM9 Knife Steel is False Advertising

It gets expensive to buy knives just to cut them up, and metallography costs even more. Support more knife steel research by going to Patreon.com/KnifeSteelNerds You get to read articles and watch videos before anyone else, participate in the Patreon community, and even get a free mug if you sign up for the highest support level.

Update: Artisan Cutlery posted to their Instagram confirming our findings:


Video

There is also a video of the following information:

AR-RPM9 Announcement and Name

AR-RPM9 was first announced in June 2020 on the CJRB Instagram, though oddly their Instagram doesn’t seem to go back that far now. I have a screenshot of it here:

CJRB is another brand owned by Artisan Cutlery. AR-RPM9 stands for “Artisan-Rare Powdered Material 9 Element Steel.” That is a very odd name so let’s break it down one element at a time. Artisan makes sense, it refers to Artisan Cutlery. But why “Artisan-Rare”? Just to have an oblique reference to AR rifles? I honestly don’t know. Then “Powdered Material” is odd, generally when we say “PM” steel that means “Powder Metallurgy” or “Particle Metallurgy” but not “powdered material.” In my original Patreon post about this steel I hypothesized that perhaps they were using weasel words for some other process that isn’t powder metallurgy but then they released a video in September 2020 where they specifically called it “powdered metallurgy” process, but we will come back to that. Then “9 Element Steel” which is a good lead-in to the composition discussion.

Composition of AR-RPM9 (Why it should actually be called AR-RPM7)

Artisan Cutlery revealed the composition of the steel in that September 2020 video. I was excited to see what it might be since they claimed to have designed a “new exclusive steel” designed specifically “with our…knives in mind.” Plus nine elements is quite a bit, so they must have gotten very creative in the design of the steel. Unfortunately, the reveal was quite underwhelming. The composition they specified was identical to the common 9Cr18MoV, the same steel as the European 1.4112, and very similar to American 440B. There were a few oddities in the description. One of the elements the video said was part of the 9 was “less than 0.4% nickel.” That is the same maximum allowable nickel content in 9Cr18MoV. Having a maximum allowable content means that it isn’t intentionally added; there is no minimum requirement. This is because nickel is present in a lot of recycled stainless steel. For example, I measured between 0.16 and 0.28% nickel in stainless powder metallurgy steels from Crucible, Carpenter, Bohler, and Uddeholm. So we are already down to 8 elements not nine.

Measurements of nitrogen, copper, nickel, cobalt, and tungsten in a range of powder metallurgy steels

Another oddity in the Instagram video was that he said there were “rare earth elements” in the steel, with elements plural so potentially we are back up to 9 or maybe even more. Before saying what those rare earth elements were, the Instagram video cut off. Rare earth elements are used in some steels and include elements like lanthanum and cerium, used for a couple different reasons in the steelmaking process. So a pretty unusual addition, especially to announce publicly, as often they are used without advertising to the public, in part because it is a trade secret and in part because they are used in very small amounts. Fortunately, Artisan Cutlery later clarified to Knife Newsroom shortly after what these elements are, and even later in December they uploaded a full version of the cutoff instagram video to YouTube. The answer was baffling: phosphorus and sulfur. Phosphorus and sulfur are not rare earth elements. I have never heard anyone say they are rare earth elements. Those are common impurity elements that are often specified with a maximum allowable content. They are not desirable, and are not considered an addition to the steel. So now we are down to 7 elements. We need to rename the steel AR-RPM7.

The only potentially relevant change is cobalt, which they said is 0.3%. 9Cr18MoV doesn’t have a cobalt specification, and 0.3% is a very small amount, so an argument could be made that it would still fit under the 9Cr18MoV spec. Cobalt is also present in a lot of recycled steel, so there is generally at least a small amount of it, though usually less than 0.3%. Furthermore, an addition of 0.3% cobalt to a steel would have a very minor effect on properties. Even with controlled testing of properties with and without 0.3% cobalt I’m not sure a metallurgist could come up with which is which. So maybe this is the change to 9Cr18MoV that they thought was enough to be a “new steel.”

I measured the composition of the steel with Optical Emission Spectroscopy (OES) and the elements were within expected ranges. Of course other trace elements were present which is also expected but I have not included them so as to not confuse anyone.

Powder Metallurgy? (Why we can’t call it AR-RPM7 either)

In my original Patreon article in June 2020 I expressed skepticism about AR-RPM9 being powder metallurgy. Artisan Cutlery already misunderstood how many elements were in their steel and apparently have no idea what a rare earth element is, so the chances they know what powder metallurgy is seemed small. Furthermore, there are several steels made in China using “Sprayform” which is a different technology than “Powder Metallurgy.” One example that has come out since AR-RPM9 is Twosun Knives YJ01-V1 which is a sprayform version of a slightly modified M390. This steel is made by Foshan Fenghe PSF (Precision Spray Form).

What is Spray Form?

Sprayform is an intermediate technology in between conventional casting and powder metallurgy. In conventional casting, the liquid steel is slowly cooled in a mold to form an ingot. The slow cooling leads to alloy segregation and large carbides. With powder metallurgy the liquid steel passes through a nozzle and is sprayed with nitrogen gas to rapidly solidify (gas atomization) the steel into fine particles (powder), which is then placed in a canister under high pressure and temperature called hot isostatic pressing (HIP) to create a solid ingot. The steel is then forged and rolled like normal. I previously wrote about powder metallurgy in this article.

Sprayform is somewhat similar to powder metallurgy in that the liquid iron is sprayed with nitrogen gas, but instead of fully solidifying, the partially solidified steel is sprayed onto a table which lowers during processing to create the entire ingot. This leads to an intermediate microstructure which is not as fine as powder metallurgy but also not as coarse as conventional steelmaking. I have an article comparing D2, sprayform D2, and powder metallurgy D2. Below are micrographs showing the difference in D2 microstructure with the three different technologies:

Conventional D2

Sprayform D2

Powder Metallurgy D2

As one more example, here are micrographs from Fenghe PSF showing their ripoff of M390 made with sprayform (right) compared with the powder metallurgy version (left):

Powder Metallurgy M390 (left) and Sprayform M390 (right)

You can see that the carbides in a sprayform steel are in between powder metallurgy and conventional. Sprayforming is done because it is lower cost vs powder metallurgy, eliminating the HIP step.

What Technology is Used for AR-RPM9?

So Shawn Houston of Triple B Handmade and I bought a couple knives from Artisan Cutlery to investigate the microstructure.

High Magnification (same as prior D2 micrographs)

AR-RPM9 Medium Magnification

Here is Sprayform D2 for comparison:

Sprayform D2 Medium Magnification

It is evident immediately that this is certainly not a powder metallurgy steel. There are many large carbides that I have never seen in any PM steel. I don’t believe that it would be possible to make a PM steel with carbides that large. With the largest carbides being around 10 microns I think sprayform is the most likely, though I could almost be talked into it being a conventionally produced steel. To compare the carbide size with 9Cr18MoV, the conventional version of this steel, we looked at edges of knives in both steels:

AR-RPM9 knife with relatively small carbides visible

9Cr18MoV knife with relatively large carbides visible

The carbides appear larger in the edge of the 9Cr18MoV knife when compared with the AR-RPM9. And the carbides in the AR-RPM9 look much too large to be powder metallurgy. So I think sprayform is the most likely production technology.

Changing the Name of AR-RPM9 to ASF7

We already discussed how the “9” should actually be a “7” in AR-RPM9, but let’s analyze the rest of the name: “Artisan-Rare Powdered Material 9 Element Steel.” We can leave the “Artisan” since that is the company selling the knives. The “rare” part I take some issue with, so we can drop that from the name. And I have discussed how “Powdered Material” is misleading so we can drop that. So we will rename the steel “Artisan Spray Form 7 Element Steel” or ASF7 for short. There, we fixed it. No more false advertising.

Properties of AR-RPM9

So now that we have discussed what AR-RPM9 likely is (and what it isn’t), what are the properties of the steel? Sprayform technology does improve toughness, though not to the extent of powder metallurgy. You can see an example with D2, sprayform D2 (PSF27), and powder metallurgy D2 (CPM-D2):

So we would expect a similar improvement over 9Cr18MoV, which would have similar toughness to 440C which I have already tested:

With 440C being around 6 ft-lbs at 59 Rc, we would expect AR-RPM9 to be in the 8-12 ft-lbs range. Nothing too spectacular but that’s what the main improvement would be over 9Cr18MoV. In terms of hardness, edge retention, and corrosion resistance, any differences would be minimal. You can read an article where I compared the edge retention of conventional and powder metallurgy 154CM to see why I think so (they performed the same). If you want to estimate the edge retention of AR-RPM9 vs other steels in my big CATRA chart you can look at 440C, or possibly a bit less.

Summary and Conclusions

AR-RPM9 is very poorly named, having only 7 elements and likely being made with sprayform but not powder metallurgy. It is essentially a sprayform version of 9Cr18MoV. Despite their claims, this steel isn’t “new” nor is it particularly exciting. The sprayform technology likely improves the toughness somewhat but wouldn’t impact much else.

The post AR-RPM9 Knife Steel is False Advertising appeared first on Knife Steel Nerds.

  •  

Matrix Steels K888 and CPM-1V

Thanks to Roman Kasé for donating the K888 and Niagara Specialty Metals for donating the CPM-1V. Thanks to my Patreon supporters for funding this study, those dollars went toward metallography and CATRA blade grinding. You can support knife steel research by visiting Patreon.com/KnifeSteelNerds

Video Version

There is also a YouTube video of the following information:

History of Matrix Steels

Matrix high speed steels were developed in the 1960’s by VASCO. I previously wrote about historical and current matrix steels in this article. The original steels came out of improved techniques for measuring the composition of the “matrix” of the steel. Some of the carbon and alloying elements go toward forming carbides, what remains is in solution in the “matrix” of the steel. Carbides help with wear resistance but are detrimental to toughness, so the metallurgists decided to make high toughness steels by taking the measured matrix composition of the best high speed steels and using that composition instead. The first was a matrix version of M2 high speed steel called VASCO-MA, and they followed that up with Matrix II, a matrix version of M42 high speed steel.

Jumping ahead to the year 2002, Crucible released CPM-1V, which is a powder metallurgy version of VASCO-MA. The steel was released to offer the highest toughness of any of their available powder metallurgy steels, even CPM-3V. In 2005, Bohler released K890, advertised as a competitor to CPM-3V, it sort of looks like a cross between CPM-1V and CPM-3V, with elevated carbon, vanadium, and cobalt when compared with CPM-1V. K888 was released at the beginning of 2024, and it is essentially CPM-1V with a cobalt addition. Cobalt is added to many high speed steels for higher hardness (with a decrease in toughness). You can read more about the effects of cobalt on steel in this article.

One intriguing thing about K888 is that Bohler is advertising that it has higher toughness at 64 Rc than their prior K890 has at 62 Rc, and that K888 sees only a small drop in toughness between 62 and 64 Rc.

Bohler’s chart of toughness for K888

Toughness drops significantly with higher hardness so the claim that K888 maintains its high toughness at such a high hardness value is exciting. For example, in testing by Hitachi of their tool steels they found that above 62 Rc the toughness of their steels drop significantly:

Hitachi toughness chart for their steels

Experiments

So I was interested to compare K888 and CPM-1V to see the effect of the cobalt addition, and I had not yet tested CPM-1V so this was a good excuse. Knifemaker Roman Kasé was able to obtain a couple small pieces of K888 for me and I got CPM-1V from Niagara Specialty Metals. CPM-1V is also now available at Alpha Knife Supply. I tested the steel for hardness, toughness, and edge retention.

Microstructure

The big benefit of matrix steels is the lower volume of carbide. Carbides are brittle particles so the less carbide found in the steel the greater the toughness. Shawn Houston did the metallography for the two steels:

CPM-1V 2050°F austenitize – 3% carbide volume

K888 2050°F austenitize – 4% carbide volume

K888 has somewhat more carbide as expected, ThermoCalc predicts 1.15% MC (vanadium carbide) and 1.84% M6C (tungsten/molybdenum carbides) in K888; CPM-1V it predicts 0.87% MC and 1.34% M6C. But the big surprise is how much bigger the carbides are in the K888. We will see if this affects the measured toughness later in the article. I have some comparable grades below such as Z-Tuff and CPM-3V, two high toughness powder metallurgy steels, as well as the conventionally produced matrix steel Caldie. CPM-1V has the finest carbides of any powder metallurgy steel I have looked at so far. You can see even more micrographs here.

Z-Tuff

CPM-3V

Caldie

Hardness

Bohler shows that K888 can be heat treated as high as 64 Rc if you use the high end of the austenitizing temperature and temper within the recommended window (blue shaded region):

I made full tempering curves for both K888 and CPM-1V. I don’t typically do full tempering curves (it takes forever), but I thought it would be useful for comparing the effect of the slightly higher carbon in the K888 as well as the cobalt addition.

The hardness I measured for K888 is roughly equal to what was shown in Bohler’s datasheet. You can see that the potential hardness is higher for K888, which is due to the cobalt addition and slightly higher carbon. However, CPM-1V is still capable of relatively high hardness. To get a better feel for the two grades, I have a comparison between the two steels on one plot:

The K888 curve is for an austenitizing temperature of 2000°F and CPM-1V is 2050°F. With the lower carbon in CPM-1V it needed a higher austenitizing temperature to have equivalent as-quenched hardness, and here the CPM-1V was slightly higher as-quenched. However, K888 saw a bigger jump in hardness with a 300°F (150°C) temper than CPM-1V did. This is “precipitation strengthening” due to small carbides coming out during tempering. The same effect happens in the high temperature range around 900°F. You can read more about precipitation strengthening, also called secondary hardening, in this article on tempering. The higher hardness after tempering is then maintained across the tempering range in K888. This is a result of the cobalt addition, which is an alloy that slows the kinetics of tempering. This is what makes cobalt useful for high speed steels, which are designed to hold their hardness at high temperature.

Toughness

I used a few different combinations of austenitizing and tempering to compare CPM-1V and K888. For K888 I compared the low and high temperature tempering with 2050°F (1120°C) along with 1000°F (540°C) and 350°F (175°C). Based on the K888 tempering chart from Bohler, the 2050-1000 combination is presumably the one they used for the 64 Rc toughness datapoint, so it was an important one to test. I also tried a lower austenitizing temperature, 2000°F (1095°C) with 400°F (200°C). For CPM-1V I used all low temperature tempering with 2000-400, 2050-300, and 2050-350. The resulting hardness and toughness is below:

The first thing that sticks out is that the CPM-1V tested significantly better than the K888. The 2050-300 treatment led to 64 Rc and 22 ft-lbs, an excellent combination of hardness and toughness. 2050-350 led to 62.5 Rc with 36 ft-lbs, again an impressive combination. The 2000-400 heat treatment, however, did not lead to an improvement in toughness when compared with 2050-350 despite the lower hardness.

For K888 the 2050-1000 heat treatment, which is presumably the heat treatment used for the 64 Rc toughness datapoint in the datasheet, had the best toughness, but it was still below the result for CPM-1V at comparable hardness. The other interesting thing was that the low temperature tempering at 350-400°F did not seem to be high enough to give the steel good toughness. This may be from the cobalt addition delaying tempering.

K888 does not look particularly impressive on the chart, though it did manage to have somewhat higher toughness than CPM-CruWear at comparable hardness. The CPM-1V was again somewhat higher than K888 around 64 Rc, showing a clearer improvement in toughness at that high hardness. At 62.5 Rc, the CPM-1V continues to look impressive, having comparable toughness to high toughness steels like Caldie, CPM-3V, and A8 mod when they are at significantly lower hardness. Z-Tuff still remains alone at the top of the chart since the 2000-400 heat treatment of CPM-1V did not lead to an improvement in toughness. However, if the CPM-1V is extrapolated to lower hardness we would expect similar toughness to Z-Tuff:

It would be interesting to test other heat treatments to see if this extrapolation to lower hardness could be achieved. Such as a 2050°F austenitize with a higher tempering temperature such as 400-500 or 1000°F to see if the toughness could be further improved in the 60-62 Rc range. Because the low tempering range was not successful for K888, modified heat treatments for lower hardness would explore lower austenitizing temperatures with the same 1000°F, or increased tempering temperatures beyond 1000°F (540°C). Presumably the toughness would remain below CPM-1V due to the larger carbides. Alternatively it would also be fun to test Z-Tuff with a lower tempering temperature of 300-350°F and see what its toughness is like at higher hardness. So far I have only tested it after tempering at 400°F.

To show how good the toughness of CPM-1V is compared to low alloy steels and stainless steels I created charts with 1V overlaid on those:

Edge Retention

I tested one CATRA knife each, Shawn Houston ground the blades after I heat treated them. Each were heat treated using an austenitizing temperature of 2050°F (1120°C) and a tempering temperature of 350°F (175°C). This resulted in 63.1 Rc for CPM-1V and 63.9 Rc for K888.

As expected the two steels are near the bottom of the chart, following the approximate edge retention of AEB-L and ApexUltra. If compensating for hardness, the two steels also approximately match CD#1 (nearly identical to Z-Tuff) and A8 Mod. So I think overall the two steels did about as well as could be hoped for high toughness powder metallurgy steels with low carbide volume and only 1% vanadium.

Summary and Conclusions

These are two matrix high speed steels based on the original matrix steel VASCO-MA, though K888 has slightly higher carbon plus a cobalt addition. The cobalt addition led to somewhat lower toughness in the K888 when compared with CPM-1V. The cobalt did lead to more tempering resistance and higher hardness, though that tempering resistance also affected its toughness, especially in the low temperature tempering range (350-400°F). CPM-1V has an excellent combination of hardness and toughness in the 62-64 Rc range, though it may be possible to achieve higher toughness in the 60-62 Rc range if we try higher tempering temperatures. K888 and CPM-1V have similar edge retention, close to AEB-L, ApexUltra, and Z-Tuff/CD#1. Overall after testing these steels CPM-1V is my preference for a steel that maintains very good toughness at high hardness. I don’t know of any knife supply companies offering K888 yet, and is apparently difficult to obtain from Bohler right now, though CPM-1V is currently available at Alpha Knife Supply.

 

The post Matrix Steels K888 and CPM-1V appeared first on Knife Steel Nerds.

  •  
❌